Mingqian
Wang
,
Zhiqiang
Ding
,
Bin
Wang
* and
Yuesheng
Li
Tianjin Key Laboratory of Composite & Functional Materials, School of Materials Science and Engineering, Tianjin University, Tianjin 300350, China. E-mail: binwang@tju.edu.cn
First published on 16th November 2022
Developing aluminum-based catalysts with high thermostability and good protic tolerance in the ring-opening polymerization (ROP) of lactide (LA) remains a great challenge, because of the decomposition of the active species under these conditions. In this contribution, a series of bipyridine bisphenolate aluminum (BpyBph-Al) complexes were synthesized and used to catalyze the ROP of LA with the assistance of an onium salt as a cocatalyst in epoxide. We disclosed the relationship between the structures of (BpyBph)Al and their catalytic performances, and thoroughly investigated the effects of polymerization conditions (including polymerization temperature, catalyst/cocatalyst and monomer/catalyst feed ratios) on LA polymerization behaviors. The (BpyBph)Al/onium binary catalytic system is of particular interest as it exhibits high thermostability and excellent tolerance to a wide range of protonic impurities, compared with the (salen)Al/onium salt. These features allowed a rapid LA polymerization under bulk and melt conditions with a very high feed ratio of [LA]:[catalyst pair]:[expoxide] = 5000:1:2. Finally, the chain initiation mechanism was further clarified by in situ NMR experiments. It was shown that a six-coordinated bis(alkoxide) aluminum complex will be generated by the (BpyBph)Al/onium salt in the presence of epoxide, which can be reversibly converted to a five coordinated (BpyBph)Al alkoxide and an alkoxide salt. The cooperative effects between the (BpyBph)Al alkoxide and the alkoxide salt were mainly responsible for rapid polymerization.
Salen-metal complexes have prevailed in the ROP of lactone, because the steric and electronic effects of the ligand can be easily modulated by chemical modification. In addition, the ONNO tetradentate structure in the salen-type ligand reduces the possibility of ligand exchange, which is beneficial for improving the stability of the catalyst.19,46–55 These features are important advantages for the development of a catalyst system that can be fine-tuned and potentially employed on an industrial scale. The pioneering studies in 1996 by Spassky reported that the (salen)Al complex with a large sterically hindered o-naphthalene bridged group could catalyze the ROP of LA to produce PLA with a high molar mass and narrow dispersity.56,57 Since then, a series of (salen)Al with structural diversity have been synthesized and used for the ROP of LA and other lactones.37,58–69 In most cases, a (salen)Al complex with an alkyl group in the axial position is used as a precursor. This precursor will react with alcohol (generally termed as an initiator) to form (salen)Al alkoxide in situ, which acts as the real active species and can initiate the ROP of LA via the coordination–insertion mechanism.66 The (salen)Al alkyl precursor is easily decomposed and finally deactivated, since the alkyl–Al bond is highly sensitive to moisture.
Metal chloride complexes are more stable than their metal alkyl counterparts, and thus may be a potential catalyst for ROP. However, there are only a few examples of the ROP of LA by metal chloride complexes. In 2001, Chisholm et al. demonstrated that aluminum chloride complexes are inactive in the ROP of LA, but they can lead to poly(propylene oxide)-b-PLA upon addition of propylene oxide.70 Although aluminum chloride complexes exhibited much lower catalytic activity than single-site LnAlOR catalysts, this fascinating work suggested that aluminum chloride will be a promising catalyst for LA polymerization. Clegg et al. found that dimeric aluminum chloride complexes can be activated by the addition of propylene oxide or cyclohexene oxide to afford efficient initiators for the ROP of LA.71 The active species was supposed to be a chloroalkoxide formed by the nucleophilic ring-opening of a coordinated epoxide. In 2017, Pang and co-workers developed air-stable and environmentally friendly salen-iron chloride for the ROP of LA and CL.72 In order to overcome the low initiation efficiency, propylene oxide was used as a solvent to activate the ring-opening reaction in situ. In particular, (salen)Fe chloride can promote the stereoselective polymerization of rac-LA via a chain-end control mechanism. Subsequently, Thomas et al. disclosed a catalyst pair consisting of a (salen)Al chloride and an onium salt.73 This binary system is of particular interest as it is the very first example of an aluminum-based catalyst active for LA polymerization at room temperature. Nonetheless, the CN bonds in salen-type ligands are sensitive to protonic impurities (such as water, alcohol and organic acid), and catalytic decrease or even complete deactivation will be observed at high temperatures and low catalyst concentration, especially in bulk polymerization, for most of the salen-Al complexes.74
Recently, we synthesized a series of bipyridine bisphenolate aluminum (BpyBph-Al) complexes and used these complexes to catalyze maleic anhydride/epoxide copolymerization for the synthesis of unsaturated polyesters.75–77 Compared with a typical (salen)Al/onium salt and Lewis pairs, the (BpyBph)Al/onium salt exhibited significantly improved tolerance to protonic impurities. Thus, the catalytic activity of the (BpyBph)Al/onium salt can be maintained at a low catalyst loading and high concentration of the chain transfer agent (100 equiv. relative to the catalyst). Increasing the catalyst's thermostability and compatibility with protonic impurities allows polymerizations at decreased catalyst concentrations, which is highly desirable to reduce cost, minimize the catalyst residue, and access high molar mass materials.78
Based on these results, the (BpyBph)Al/onium salt binary catalysts were further used to catalyze the ROP of LA in this work (Scheme 1). We disclosed the relationship between the structures of (BpyBph)Al and their catalytic performances, and investigated the effects of polymerization conditions (including polymerization temperature, catalyst/cocatalyst and monomer/catalyst feed ratios) on LA polymerization behaviors. Compared with the (salen)AlCl/onium salt, the (BpyBph)Al/onium salt exhibited superior performance in LA polymerization. The catalytic activity of (BpyBph)AlCl/PPNCl is about 4–8 fold higher than those of (salen)AlCl/PPNCl at 180 °C. Besides, the (BpyBph)Al complexes showed excellent tolerance to a wide range of protonic impurities, compared with (salen)Al complexes. These features allowed a rapid LA polymerization under bulk and melt conditions. Finally, the chain initiation mechanism was clarified by in situ NMR experiments.
1H and 13C {1H} NMR spectra were recorded on a Bruker Avance III spectrometer (400 MHz for 1H NMR and 100 MHz for 13C NMR) at room temperature in CDCl3. The molar mass and dispersity (Đ) of copolymers were determined by size exclusion chromatography (SEC) at 40 °C with a flow rate of 1.0 mL min−1, using THF as the eluent on an Agilent PL-SEC 50 instrument coupled with a refractive index (RI) detector with respect to polystyrene (PS) standards. The columns included a Plgel guard 50 × 7.5 mm column, a PLgel mixed-B 300 × 7.5 mm column and a PLgel mixed-C 300 × 7.5 mm column. Samples for the SEC test were filtered through a 0.22 μm PTFE filter. The matrix-assisted laser desorption/ionization time-of-flight mass spectra of typical polymer samples are performed on a Bruker Autoflex III mass spectrometer in linear, positive ion mode, using trans-2-[3-(4-tert-butylphenyl)-2-methyl-2-propylidene] malononitrile (DCTB) and 2,5-dihdyroxybenzoic acid (DHB) as a matrix, and THF as a solvent.
Entry | Cat. | Conv.b (%) | TOFc (h−1) | M n,theod (kDa) | M n,expe (kDa) | Đe |
---|---|---|---|---|---|---|
a Unless otherwise stated, the ROPs were carried out in 0.5 mL of propylene oxide with 10 mmol Al complex at 80 °C for 0.5 h, [LA]0 = 2.0 M, [LA]:[Al]:[PPNCl] = 100:1:1. b Monomer conversion was determined by 1H NMR. c TOF (turnover frequency) = mol of anhydride consumed × mol. of catalyst × h−1. d The theoretical number-averaged molar mass Mn,theo was calculated by Mn,theo = [LA]/[I] × % conv. (LA) × M(LA). e The experimental number-averaged molar mass Mn,exp and dispersity (Đ) were determined by SEC. The Mn,exp value obtained by SEC was further corrected by a correcting factor of 0.58.81 f The polymerization was conducted at room temperature. g In the absence of the PPNCl cocatalyst, polymerization time = 8 h. h [LA]:[Al]:[PPNCl] = 100:1:0.5, polymerization time = 0.5 h. i [LA]:[Al]:[PPNCl] = 100:1:2, polymerization time = 0.25 h. j [LA]:[Al]:[PPNCl] = 100:1:5, polymerization time = 0.25 h. | ||||||
1 | 1/PPNCl | 96 | 192 | 13.8 | 6.7 | 1.22 |
2 | 2/PPNCl | 80 | 160 | 11.5 | 5.2 | 1.26 |
3 | 3/PPNCl | 85 | 170 | 12.3 | 6.3 | 1.24 |
4 | 4/PPNCl | 82 | 164 | 11.8 | 5.8 | 1.28 |
5 | 5/PPNCl | 90 | 180 | 13.0 | 5.9 | 1.30 |
6 | 6/PPNCl | 72 | 144 | 10.4 | 5.0 | 1.25 |
7 | 7/PPNCl | 75 | 150 | 10.8 | 5.2 | 1.27 |
8 | 8/PPNCl | 78 | 156 | 11.2 | 5.0 | 1.21 |
9f | 5/PPNCl | 80 | 16 | 11.5 | 5.5 | 1.22 |
10g | 5/— | 15 | 1.9 | 2.2 | — | — |
11h | 5/PPNCl | 36 | 72 | 5.2 | 2.1 | 1.22 |
12i | 5/PPNCl | 81 | 324 | 11.7 | 4.6 | 1.35 |
13j | 5/PPNCl | 92 | 638 | 13.3 | 1.8 | 1.57 |
The electronic effect and steric hindrance in Al complexes significantly affect the polymerization rate as well. Substituting t-Bu groups (complex 3) with more electron-donating –OCH3 groups (complex 4) resulted in a slight decrease in catalytic activity (entry 4, Table 1), while introducing electron-withdrawing fluorine atoms in the para-position (complex 5) increase the catalytic activity to some extent (entry 5, Table 1). Here, we suppose that the electron-withdrawing group will increase the Lewis acidity of the metal center, which facilitates its coordination with LA and activation of the monomer. 6/PPNCl was proved to be less active than 3/PPNCl (TOF: 170 vs. 144 h−1) (entry 6, Table 1). The bulky steric hindrance around aluminum also will hinder the coordination of the active aluminum complex to the next coming LA monomer. Substituting the axial –Cl group in complex 4 with OAc− (complex 7) and TFA− (complex 8) did not affect the polymerization rate (entries 7 and 8, Table 1), and we observed very similar catalytic activity for these three complexes in the presence of PPNCl. We envisioned that the active species formed in situ by 4/PPNCl, 7/PPNCl and 8/PPNCl in the presence of epoxide exhibited similar activity toward lactide (see below). The ROP of LA catalyzed by 5/PPNCl could proceed smoothly at room temperature (entry 9, Table 1), but the polymerization rate dramatically decreased. The resultant PLAs exhibited monomodal dispersity.
The LA polymerization follows first-order kinetics, as evidenced by the good linearity between ln[LA]0/[LA]t and reaction time (Fig. S1†). Notably, the experimental Mn,exp values for the resultant polyester samples are approximately half of the theoretical values (Mn,theo), suggesting the formation of two polymeric chains per metal center. This is in contrast to the LA copolymerization catalyzed by (salen)Al alkoxide, where only one polymer chain is initiated per metal center.
The effect of the [Al]:[PPNCl] feed ratio on LA polymerization was further investigated, considering that the amount of PPNCl will be crucial to generate a potent active species. We observed a slow polymerization by using complex 5 alone and without PPNCl as a cocatalyst. Only 15% of LA was converted by complex 5 after 8 h (entry 10, Table 1). Introducing 0.5 equiv. of PPNCl led to a more rapid polymerization with a LA conversion of 36% in 0.5 h, affording PLA with monomodal dispersity and Mn,exp approximately half of the theoretical value (entry 11, Table 1). The polymerization would be accelerated by further increasing the ratio of [PPNCl]:[Al] to 2:1 and 5:1 (entries 12 and 13, Table 1) with LA conversions of 81% and 92% in 0.25 h, respectively. However, the resultant PLAs exhibited much lower Mn,exp than Mn,theo/2 and broader dispersity. It was envisioned that a high quantity of PPNCl favored substantial chain transfer reactions. In agreement with previous observations with the (porphyrin)AlCl complex, the presence of excess [PPN]Cl can cause a displacement of the alkoxide anion by the chloride, generating the new onium salt [PPN]OR and ultimately leading to the formation of the corresponding bis(alkoxide) complexes. As the polymerizations are conducted in propylene oxide, excess PPNCl can lead to the formation of several [PPN]OR species, finally resulting in PLA with a lower molar mass.
To further highlight the synergistic effect between the BpyBph-Al complex and PPNCl, we further monitored the LA polymerization catalyzed by PPNCl alone at 80 °C with a feed ratio of [LA]:[PPNCl] = 100:1 (Fig. S2†). There is an induction period for PPNCl catalyzed LA polymerization. We did not detect LA consumption within 90 min, and a low LA conversion was observed at 120 min. PPNCl exhibited a very different catalytic behavior from the BpyBph-Al/PPNCl binary system, supporting that (BphBpy)AlCl and PPNCl cooperatively catalyze LA polymerization. PPNCl mainly served as a Lewis base to initiate the ring-opening reaction of epoxide that was activated by (BphBpy)AlCl (see below).
Entry | Cat. | T (°C) | t (h) | Conv.b (%) | TOFc (h−1) | M n,theod (kDa) | M n,expe (kDa) | Đe |
---|---|---|---|---|---|---|---|---|
a Unless otherwise stated, the ROPs were carried out in 2.5 mL of propylene oxide with 10 mmol Al complex, [LA]0 = 2.0 M, [LA]:[Al]:[PPNCl] = 500:1:1. b Monomer conversion was determined by 1H NMR. c TOF (turnover frequency) = mol. of anhydride consumed × mol. of catalyst × h−1. d The theoretical number-averaged molar mass Mn,theo was calculated by Mn,theo = [LA]/[I] × % conv. (LA) × M(LA). e The experimental number-averaged molar mass Mn,exp and dispersity (Đ) were determined by SEC. The Mn,exp value obtained by SEC was further corrected by a correcting factor of 0.58.81 f The polymerization was conducted under bulk and melt conditions with a feed ratio of [LA]:[5]:[PPNCl]:[1,2-epoxyhexane] = 2000:1:1:2. g The polymerization was conducted under bulk and melt conditions with a feed ratio of [LA]:[5]:[PPNCl]:[1,2-epoxyhexane] = 5000:1:1:2. | ||||||||
1 | 1/PPNCl | 80 | 5 | 93 | 93 | 67.0 | 19.1 | 1.28 |
2 | 2/PPNCl | 80 | 5 | 84 | 84 | 60.5 | 15.7 | 1.27 |
3 | 5/PPNCl | 80 | 5 | 88 | 88 | 63.4 | 18.0 | 1.25 |
4 | 1/PPNCl | 130 | 3 | 67 | 112 | 48.2 | 9.8 | 1.44 |
5 | 2/PPNCl | 130 | 3 | 75 | 125 | 54.0 | 10.6 | 1.42 |
6 | 5/PPNCl | 130 | 3 | 85 | 142 | 61.2 | 14.2 | 1.44 |
7 | 1/PPNCl | 180 | 2 | 12 | 30 | 0.8 | — | — |
8 | 2/PPNCl | 180 | 2 | 26 | 65 | 18.7 | — | — |
9 | 5/PPNCl | 180 | 2 | 98 | 245 | 70.6 | 13.8 | 1.53 |
10f | 5/PPNCl | 200 | 6 | 93 | 310 | 267.8 | 72.5 | 1.28 |
11g | 5/PPNCl | 200 | 12 | 87 | 363 | 626.4 | 115.1 | 1.31 |
Entry | Cat. | T (°C) | Protic agent | Equiv. to [Al-PPNCl] | Conv.b (%) | TOFc (h−1) | M n,expd (kDa) | Đd |
---|---|---|---|---|---|---|---|---|
a Unless otherwise stated, the ROPs were carried out in 2.5 mL of propylene oxide with 10 mmol Al complex at 80 °C for 5 h, [LA]0 = 2.0 M, [LA]:[Al]:[PPNCl] = 500:1:1. b Monomer conversion was determined by 1H NMR. c TOF (turnover frequency) = mol. of anhydride consumed × mol. of catalyst × h−1. d The experimental number-averaged molar mass Mn,exp and dispersity (Đ) were determined by SEC. The Mn,exp value obtained by SEC was further corrected by a correcting factor of 0.58.81 | ||||||||
1 | 5/PPNCl | 80 | BnOH | 10 | 92 | 92 | 5.2 | 1.26 |
2 | 5/PPNCl | 80 | BnOH | 20 | 91 | 91 | 3.0 | 1.24 |
3 | 5/PPNCl | 80 | BnOH | 50 | 89 | 89 | 1.5 | 1.28 |
4 | 5/PPNCl | 80 | BnOH | 100 | 85 | 85 | — | — |
5 | 5/PPNCl | 80 | iPrOH | 50 | 95 | 95 | 1.3 | 1.21 |
6 | 5/PPNCl | 80 | H2O | 50 | 86 | 86 | 1.0 | 1.18 |
7 | 5/PPNCl | 80 | Maleic acid | 50 | 85 | 85 | 1.1 | 1.19 |
8 | 1/PPNCl | 80 | BnOH | 50 | 45 | 45 | 0.7 | 1.20 |
9 | 1/PPNCl | 80 | BnOH | 100 | 15 | 15 | — | — |
10 | 1/PPNCl | 80 | Maleic acid | 50 | 35 | 35 | 0.6 | 1.30 |
11 | 2/PPNCl | 80 | BnOH | 50 | 57 | 57 | 0.9 | 1.23 |
12 | 2/PPNCl | 80 | BnOH | 100 | 25 | 25 | — | — |
13 | 2/PPNCl | 80 | Maleic acid | 50 | 40 | 40 | 0.5 | 1.26 |
The catalytic activities of 1/PPNCl, 2/PPNCl and 5/PPNCl increased to some extent by elevating the polymerization temperature from 80 to 130 °C (entries 1–6, Table 2). However, the activities of 1/PPNCl and 2/PPNCl sharply decreased when further increasing the temperature to 180 °C (entries 7 and 8, Table 2). The LA conversion after 2 h was 12% and 26%, respectively for 1/PPNCl and 2/PPNCl at 180 °C. This result may be ascribed to the decomposition of active species derived from (salen)Al/PPNCl, which can be observed in the ring-opening copolymerization of cyclic anhydride and epoxide at high temperatures.83 By contrast, we observed more rapid polymerization by using 5/PPNCl at 180 °C, and LA was consumed almost completely in 2 h (entry 9, Table 2). These results clearly indicated that the 5/PPNCl pair exhibited much higher thermostability than 1/PPNCl and 2/PPNCl. Here, we supposed that the bipyridine (bpy) bridging group with an extended π-conjugate may be responsible for the high thermostability of the (BpyBph)Al complex. 5/PPNCl could efficiently promote the ROP of LA even under bulk and melt conditions by using 1,2-epoxyhexane with a high boiling point as a co-initiator (entries 10 and 11, Table 2). It was noted that the molar mass of PLA decreased, and the dispersity became broad as the polymerization temperature increased, indicative of serious side reactions (such as transesterification and chain transfer reactions) at high temperatures.
Compared with 1/PPNCl and 2/PPNCl pairs, 5/PPNCl shows good tolerance to protic agents, such as benzyl alcohol (BnOH), isopropanol (iPrOH), water (H2O) and maleic acid. We first chose BnOH to mimic protic impurity and investigated the variation in the catalytic activity of 5/PPNCl under different BnOH loading dosages. We did not observe an obvious decay in catalytic activity by gradually increasing the [BnOH]:[catalyst pair] feed ratio from 10:1 to 100:1 (entries 1–4, Table 3). However, the molar mass of the resultant PLA decreased with an increase of the [BnOH]:[catalyst pair] feed ratio, suggesting that BnOH could serve as a chain transfer agent. The ROPs were further conducted using 5/PPNCl in the presence of 50 equiv. of iPrOH, H2O and maleic acid, respectively (entries 5–7, Table 3). All the copolymerization could proceed smoothly without obvious decay of catalytic activity. These results clearly indicated that 5/PPNCl exhibits good tolerance to a wide range of protic reagents. By contrast, the activity for 1/PPNCl (from 93 to 45 h−1) and 2/PPNCl (from 84 to 57 h−1) substantially decreased in the presence of 50 equiv. of BnOH (entries 8 and 11, Table 3). We observed a further decrease of activity for these two catalysts by increasing the [BnOH]:[catalyst pair] feed ratio to 100:1 (entries 9 and 12). Introducing 50 equiv. of maleic acid as a protic impurity also resulted in a decline in activity for 1/PPNCl and 2/PPNCl, respectively (entries 10 and 13).
Scheme 2 Proposed mechanism of chain initiation by the (BpyBPh)AlCl/PPNCl catalyst pair according to in situ1H and 19F NMR spectroscopy. |
When 3 equiv. of BO was added to 4/PPNTFA or 8/PPNCl, only 1 equiv. of BO underwent a ring opening, and the rest of the BO was still intact even after 24 h (Fig. 1a, Fig. S5, S6 and Tables S1, S2†). 1H and 19F NMR spectroscopy indicated the formation of a five-coordinated Al alkoxide complex INT3 and free PPNTFA (Fig. S3 and S5†). Notably, the six-coordinate complex INT2 was not detected on the NMR time scale. We deduced that the stronger nucleophilicity of TFA− in INT1 resulted in tight coordination with the Al center and that the first equiv. of BO underwent ring opening by the departing Cl−. Once INT2 formed, TFA− dissociated rapidly, and INT3 formed spontaneously, because TFA− is a better leaving group than alkoxide. In the presence of a larger excess of BO (5 equiv. relative to 4/PPNTFA), coordination of INT3 with BO and subsequent nucleophilic attack by TFA− afforded the six-coordinate bis(alkoxide) Al complex INT5 (Fig. 1b). Additionally, the upfield shift of the TFA− peak implied that TFA− was involved in the nucleophilic attack on BO (Fig. S3D†). Notably, the ring opening of PO during chain initiation occurred on both sides of the Al-ONNO coordination plane, and the six-coordinated bis(alkoxide) Al complex INT5 was finally generated (Scheme 2).
We hypothesized that there will be an association/dissociation equilibrium between a six-coordinated bis(alkoxide) Al complex and a mixture consisting of five-coordinated (BpyBph)Al alkoxide and [PPN]+ alkoxide (PPNOR). During chain propagation, the competitive coordination of the LA monomer with an aluminum center can facilitate the dissociation of the six-coordinated bis(alkoxide) Al complex. The five-coordinated (BpyBph)Al alkoxide alone exhibits extremely low catalytic activity toward LA polymerization, and thus it mainly acts as a Lewis acid and activates the LA monomer by coordination in the vacant axial position. The PPNOR can act as a Lewis base and induce the ring-opening of the activated LA via nucleophilic attack. The cooperative effects between (BpyBph)Al alkoxide and PPNOR are mainly responsible for the rapid polymerization. Once the activated LA is ring-opened by PPNOR, a new six-coordinated bis(alkoxide) Al complex will be generated that can be converted to five-coordinated (BpyBph)Al alkoxide and PPNOR again. Then, the next LA monomer is inserted into the polymer chain with the assistance of the (BpyBph)Al alkoxide/PPNOR pair. The ROP of LA proceeds via coordination anionic polymerization by repeating the above reaction cycle.
It is assumed that each individual alkoxide in the active six-coordinated bis(alkoxide) Al complex could initiate one polymer chain. Finally, two polymer chains were initiated by per metal catalyst. This point could be supported by the experimental results that Mn,exp is approximately Mn/2 (see Table 1). To find more evidence for this mechanism, the PLA sample obtained from 8/PPNCl was further analyzed by matrix-assisted laser desorption/ionization time-of-flight (MALDI-TOF) mass spectrometry. We could observe two populations in the mass spectra, which were attributed to linear PLA with chloroalkoxide and a trifluoroacetic alkoxide chain end, respectively (Fig. 2). In addition, the chloroalkoxide and trifluoracetic alkoxide chain ends could be further confirmed by 1H, 13C and DEPT(135°) NMR spectra (Fig. S7–S9†). These results strongly indicated that the six-coordinated bis(alkoxide) Al complex was the real active species for LA polymerization. Each of the alkoxide groups, which was derived from the axial group in the Al complex and the nucleophilic anion in the PPN salt, respectively, could initiate one polymer chain. The MALDI-TOF MS data also suggested that propylene oxide is only ring-opened to form active species but will not be inserted into the active polymer chain during propagation.
As mentioned above, the (BpyBph)Al chloride complex could promote LA polymerization in the presence of propylene oxide without an onium salt as a cocatalyst, resulting in a very slow polymerization with a LA conversion of 15% after 8 h at 80 °C. The chain initiation mechanism was thus further investigated by an in situ NMR experiment. We did observe the formation of five-coordinated neutral Al alkoxide species after mixing complex 4 alone with BO (Fig. S10†). This five-coordinated Al alkoxide cannot be converted to the six-coordinated bis(alkoxide) Al complex in the presence of 5 equiv. of BO without the PPNCl cocatalyst. Thus, the five-coordinated neutral Al alkoxide was the active species that can initiate the ROP of LA via the coordination–insertion mechanism (Scheme 3). Such a “co-initiation mechanism” by epoxides was also found in the LA polymerization catalyzed by aluminum-, titanium- and iron chloride systems.71,72
Scheme 3 Coordination–insertion mechanism for chain propagation initiated by (BpyBph)AlCl without the PPNCl cocatalyst. |
In situ NMR experiments and end group analysis by MALDI-TOF MS revealed that a highly active six-coordinated bis(alkoxide) aluminum complex was formed by reaction of the (BpyBph)Al/onium salt with epoxide, and it will be transformed into a neutral five-coordinated aluminum alkoxide and a PPN+ alkoxide. The five-coordinated aluminum alkoxide (Lewis acid) and PPN+ alkoxide (Lewis base) cooperatively catalyze the ROP of LA, finally leading to very rapid LA polymerization. Each individual alkoxide in the active six-coordinated bis(alkoxide) Al complex could initiate one polymer chain, and thus two polymer chains were initiated per metal catalyst.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d2py01273a |
This journal is © The Royal Society of Chemistry 2023 |