aSchool of Applied Physics and Materials, Wuyi University, Jiangmen 529020, PR China. E-mail: wangfux91@126.com
bMOE of the Key Laboratory of Bioinorganic and Synthetic Chemistry, The Key Lab of Low-carbon Chem & Energy Conservation of Guangdong Province, School of Chemistry, Sun Yat-Sen University, Guangzhou 510275, PR China
First published on 19th May 2023
Molybdenum trioxide (MoO3) is emerging as a hugely competitive cathode material for aqueous zinc ion batteries (ZIBs) for its high theoretical capacity and electrochemical activity. Nevertheless, owing to its undesirable electronic transport capability and poor structural stability, the practical capacity and cycling performance of MoO3 are yet unsatisfactory, which greatly blocks its commercial use. In this work, we report an effective approach to first synthesise nanosized MoO3−x materials to provide more active specific surface areas, while improving the capacity and cycle life of MoO3 by introducing low valence Mo and coated polypyrrole (PPy). MoO3 nanoparticles with low-valence-state Mo and PPy coating (denoted as MoO3−x@PPy) are synthesized via a solvothermal method and subsequent electrodeposition process. The as-prepared MoO3−x@PPy cathode delivers a high reversible capacity of 212.4 mA h g−1 at 1 A g−1 with good cycling life (more than 75% capacity retention after 500 cycles). In contrast, the original commercial MoO3 sample only obtains a capacity of 99.3 mA h g−1 at 1 A g−1, and a cycling stability of 10% capacity retention over 500 cycles. Additionally, the fabricated Zn//MoO3−x@PPy battery obtains a maximum energy density of 233.6 W h kg−1 and a power density of 11.2 kW kg−1. Our results provide an efficient and practical approach to enhance commercial MoO3 materials as high-performance cathodes for AZIBs.
As an innovative energy storage device, AZIBs currently have limited range of materials suitable as cathode materials for zinc ion storage.17 They are mainly consist of manganese-based oxides,18 vanadium-based oxides,19 molybdenum-based oxides,1 Prussian blue and its analogues,20 and organic oxides.21 Among them, molybdenum trioxide (MoO3) has the advantages of high abundance,22 low toxicity and easy recovery,23 as well as its multivalent states and two-dimensional layered structure.24 Nevertheless, MoO3 suffers from a serious drawback that it tends to dissolve in neutral or weakly acidic electrolytes to destroy its structure,25 resulting in low actual capacity and poor cycling stability.26 In previous studies, the electrochemical performance of electrode materials have been generally boosted by means of modifications such as morphology modulation,27 interfacial engineering,28 valence modulation,29 doping and coating,30 and composites.31 As an instance, Liu et al. reported that MoO3 can exhibit an initial discharge capacity of 120 mA h g−1, but its capacity decreases sharply over 5 cycles of charging/discharging, mainly due to the structure damage.26 Liu et al. used a surface engineering to avoid the structure damage of electrode material through coating a layer of Al2O3 on the surface of MoO3. Through the DFT calculations, MoO3−x obtain a lower Gibbs free energy of Zn2+ adsorption on the surface of MoO3−x, indicating that the desorption of Zn2+ on MoO3−x is thermodynamically more beneficial and its adsorption/desorption of Zn2+ is more reversibility. In addition, it leads to a narrower of the band gap between the valence band and the conduction band, which facilitates the excitation of charge carriers to the conduction band and thus improves the electrical conductivity of MoO3−x.32 The assembled Zn//P-MoO3−x@Al2O3 battery shows improved cycling stability. The capacity retention of Zn//P-MoO3−x@Al2O3 battery was 69.2% over 100 cycles, which is better than that of that of Zn//P-MoO3−x battery (only 40.8%).32 He et al. developed an effective strategy for quasi-solid PVA/ZnCl2 gel electrolyte to stabilize MoO3 nanowires instead of aqueous electrolyte, and the capacity retention of the assembled MoO3//Zn battery reach to 70.4% in gel electrolyte over 400 cycles, but only 27.1% in aqueous electrolyte.33 In addition, Zhang et al. developed WP-MoO3 electrodes by a water-proton co-pre-insertion strategy. WP-MoO3 electrode achieve selective hydrated proton insertion by using water molecules between the layers to increase the insertion energy barrier of zinc ions by blocking the transport path of zinc ions. Based on the above merits, the capacity retention of the prepared battery is 83% after 1000 cycles.34 Despite the impressive progress of these works, there is still room to enhance the capacity and cycle stability of MoO3. Moreover, exploring simpler and practical ways to boost the electrochemical performance of MoO3 electrodes remains a meaningful challenge.35
In this work, we focus on improving the capacity and cycling stability of commercial MoO3 through a simple and effective approach. Low-valent state enriched and polymer coated MoO3 electrode materials (MoO3−x@PPy) are synthesized by a simple solvothermal method and subsequent electrodeposition process. The reactivity and structural stability of MoO3−x@PPy electrodes are boosted with the help of low-valence-state Mo introduction and coating strategies. Firstly, the solvothermal reaction allows the MoO3 particles to be nanosized to obtain more active sites, while the introduction of low-valent molybdenum improves the reactivity of the electrode material. Secondly, the coated PPy layer improves the stability of the electrode material in the electrolyte. Combing the above advantages, the assembled Zn//MoO3−x@PPy battery obtain a high reversible capacity of 212.4 mA h g−1 at 1 A g−1 and favorable cycle life of 75% capacity retention over 500 cycles, while that of Zn//MoO3 battery is only 99.3 mA h g−1 at 1 A g−1 and 10% capacity retention over 500 cycles. Moreover, the fabricated Zn//MoO3−x@PPy battery exhibits a maximum energy density of 233.6 W h kg−1 and power density of 11.2 kW kg−1.
Fig. 1 (a) Schematic illustration of the synthesis of MoO3−x@PPy electrode material. (b and d) SEM images of MoO3−x electrode material. (c and e) SEM images of MoO3−x@PPy electrode material. |
To further investigate the microstructure and crystal type of the material, the synthesized material was characterized by TEM and XRD. Fig. S2† shows a TEM image of commercial MoO3 showing a particle size of approximately 150 nm. In addition, a lattice stripe of 0.133 nm is visible in the HRTEM image of MoO3, which corresponds to the (202) crystal plane of MoO3 (JCPDF # 05-0508), while the calibrated diffraction points in selected electron diffraction (SAED) pattern of the MoO3 material correspond to the to the (150), (210) and (110) crystal planes of MoO3 (JCPDF # 05-0508). Fig. 2a and b shows a TEM image of MoO3−x, showing a particle size of approximately 50 nm, which is much smaller than the commercial MoO3 material and in line with the SEM results. However, SAED pattern of the MoO3−x material shows two distinct diffraction rings corresponding to the (−321) crystal plane of MoO2 (JCPDS # 32-0671) and the (041) crystal plane of MoO3 (JCPDF # 05-0508), indicating the introduction of low-valent-state Mo after solvothermal reaction. Fig. 2c shows a TEM image of MoO3−x@PPy showing a thin film outside the MoO3−x material, demonstrating that PPy is encapsulated on the surface of the MoO3−x electrode material. Subsequently, the elemental distribution in the MoO3−x@PPy material was analyzed by energy density spectroscopy (EDS). The results display that the O, Mo and N elements are evenly dispersed on the electrode material, again proving that PPy is evenly coated on the MoO3−x electrode material. The crystallization pattern of the prepared materials was investigated more thoroughly by XRD test. Fig. 3a shows the XRD patterns of commercial MoO3, MoO3−x, and MoO3−x@PPy materials. It is noteworthy that the MoO3−x sample synthesized after the solvothermal reaction contains a large number of characteristic peaks (−111), (200), and (211) of MoO2 (JCPDS # 32-0671) peaks and a small number of characteristic peaks (110), (040), and (112) of MoO3, while only characteristic peaks of MoO3 (JCPDF # 05-0508) are present in the commercial MoO3, which implies the successful introduction of low-valent-state Mo in the commercial MoO3 by the solvothermal reaction. In addition, the XRD pattern of MoO3−x@PPy material after electrodeposition of PPy shows a decrease in peak intensity, but characteristic peaks of MoO2 (−111), (200), (211) and MoO3 (112) still can be found in the sample, which indicates that the coated amorphous PPy do not change the crystal structure, which is in line with the results of TEM test. Furthermore, XPS was utilized to analyses the valence and elemental composition of the material. As shown in Fig. 3b and S3b,† the Mo 3d spectrum of commercial MoO3 matches the two characteristic peaks of 3d5/2 and 3d3/2 of Mo6+ at 232.75 and 235.93 eV respectively,36 indicating that molybdenum is predominantly present in commercial MoO3 at +6 valence. However, the MoO3−x sample produced by solvothermal reduction with ethylene glycol showed two additional peaks in its Mo 3d spectrum. Of these, 230.43 and 233.13 eV correspond to the 3d3/2 and 3d5/2 characteristic peaks of Mo4+.37 The presence of Mo4+ indicates the introduction of low-valence-state Mo into the material. Furthermore, according to the analysis of the XPS test, the two characteristic peaks of Mo6+ are still found at 232.64 and 235.41 eV, which implies that the commercial MoO3 has not been completely reduced to MoO2. Fig. S3a† displays the XPS survey spectra of MoO3 and MoO3−x@PPy electrode material, which shows that only the material of MoO3@PPy contains N elements, indicating the successful coated of PPy.38 Also Fig. S3c† shows the Mo 3p spectra of MoO3 and MoO3−x@PPy. The Mo 3p peak is sharper for MoO3, while the distinct hump at 397.5 eV in the Mo 3p XPS spectrum of MoO3−x@PPy further confirms the presence of N on the MoO3−x@PPy surface.39 The O 1s spectra of the MoO3 and MoO3−x samples in Fig. 3c show that for 530.8 ± 0.1 eV (green area fraction) the binding energy component is derived from the lattice oxygen (Oa) of MoO3, for the MoO3−x sample the peak at 532.2 ± 0.1 eV (yellow area fraction) is associated with a chemically absorbed oxygen site (Oc).38 Fig. 3d shows the Fourier transform infrared spectra (FT-IR) of MoO3−x and MoO3−x@PPy electrode materials. The FT-IR spectra of both electrode materials show the core characteristic peaks of molybdenum oxide (Mo–O–Mo), while the main characteristic peaks of PPy (CC and C–N) are also observed in the MoO3−x@PPy electrode,40 again demonstrating that PPy was successfully coated on the surface of the MoO3−x material.
Fig. 2 (a) TEM and (b) HRTEM images of MoO3−x material (inset the SAED pattern). (c) TEM image of MoO3−x@PPy material (inset the SAED pattern). (d) The corresponding area EDS mapping. |
To further investigate the effects of low-valence-state Mo introduction and PPy coating strategies on the zinc storage property of commercial MoO3 materials, a series of AZIBs based on the synthesized MoO3, MoO3−x, and MoO3−x@PPy materials MoO3 as cathode, zinc plate as anode and 2 M ZnSO4 as electrolyte were assembled. First, we optimised the thickness of the electrodeposition PPy layers. As shown in Fig. S4,† its electrochemical property decreases as the number of deposition cycles increases, indicating that too thick PPy will hinder MoO3−x from participating in the electrochemical reaction. However, PPy layer with appropriate thickness (2 cycles of electrodeposition) can not only stabilize the structural stability of MoO3−x in electrolyte, but also provide additional zinc storage performance. Fig. 4a shows the CV curves of assembled Zn//MoO3, Zn//MoO3−x, and Zn//MoO3−x@PPy batteries at 20 mV s−1 within the operating window of 0.2–1.3 V.
The graph clearly shows that the CV curves of the three batteries are almost identical in shape, but the current response signal gradually enlarges as the introduction of the low-valence-state Mo and the PPy coating, indicating that their zinc storage performance gradually enhanced. Then, the GCD curves in Fig. 4b shows more clearly that the Zn//MoO3−x@PPy battery achieves a highest discharge capacity of 212.4 mA h g−1 (based on the mass of the cathode active material) at 1 A g−1, while that of Zn//MoO3−x and Zn//MoO3 batteries are only 181.7 mA h g−1 and 99.3 mA h g−1, respectively. These results demonstrate that the introduce of low-valence-state Mo and PPy coating strategies can boost the Zn storage capacity of commercial MoO3. Furthermore, the rate performance of the fabricated three kinds of batteries was characterized at different current densities, illustrated in Fig. 4d, where the Zn//MoO3−x@PPy shown highest capacities at all currents. The reversible specific capacities of Zn//MoO3−x@PPy battery can reach 212.4 mA h g−1 to 73.3 mA h g−1 at the current density of 1 to 10 A g−1, respectively. In particular, Zn//MoO3−x@PPy battery exhibited 35% capacitance retention even at a high current density of 10 A g−1. By contrast, Zn//MoO3 battery achieved specific capacities of 99.3 mA h g−1 to 10.5 mA h g−1 at 1 to 10 A g−1, respectively. Its rate property is only 10.6%, again indicating that the low-valence-state Mo introduction and PPy coating strategies can boost the capacity and rate property of commercial MoO3 for zinc storage. Much encouragingly, the Zn//MoO3−x@PPy battery maintained 75% capacity retention over 500 cycles, while that of Zn//MoO3 and Zn//MoO3−x batteries were not high, 61% and 10%, respectively, indicating that coating with a corrosion resistant polymer coating is a very simple and practical way to enhance the stability of electrode materials (Fig. 4c). It is worth noting that the specific capacity of MoO3 is improved over the first 100 cycles, which might attribute to the continuous activation of the electrode due to the surface chemical reactions between MoO3 and the ZnSO4 electrolyte.41 Energy density and power density are the two vital parameters for evaluating the energy storage capacity of batteries. As shown in Fig. 4e, the fabricated Zn//MoO3−x@PPy battery obtained an energy density of up to 233.6 W h kg−1 (power density of 1.1 kW kg−1) and the maximum power density of 11.2 kW kg−1 (energy density of 80.6 W h kg−1), exceed those of some newly published aqueous batteries, as shown in Table 1. This satisfactory energy density and power density are expected to enable our designed Zn//MoO3−x@PPy battery to become a more practical alternative power source.
The electrochemical kinetics of the fabricated electrode were further investigated by conducting CV measurements at various scan rates ranging from 1 to 10 mV s−1 (displayed in Fig. 5a and S5†). As can clearly be seen the figure of the CV curve at any scan rates is essentially the same, but the peaks are slightly shifted. The diffusion and pseudocapacitance behaviour of the battery during the charge/discharge cycle was distinguished by adjusting the scan rate to correspond to the response of the peak current. In the case of a dominant battery behaviour, the relationship between peak current i and scan voltage v follows a power function of 0.5, indicating that diffusion plays an important role throughout the process. When analyzing battery behavior during charge/discharge cycles, it is possible to distinguish between diffusive and pseudo-capacitive behavior by adjusting the scan rate to match peak current response. In cases where the process is dominated by capacitance, peak current i varies linearly with scanning voltage v. To determine the presence of pseudo-capacitive behavior, researchers can calculate the b value using the equation i = avb. This allows for a more accurate understanding of electrode material behavior during charging and discharging. When the value of b equals 0.5, the electrode material displays battery characteristics. If the value of b falls among 0.5 to 1, both battery and pseudocapacitive properties can be observed in the electrode material. When b is greater than or equal to 1, the electrode material mainly displays pseudocapacitive behavior. Fig. 5b displays the fitted CV curves for the MoO3−x@PPy samples at different scan rates. It is noteworthy that the calculated b value of the reduction peak is 0.79, suggesting that a blend of both diffusion-controlled and capacity-based kinetic phenomena occurred. To determine the pseudo-capacitance contribution of MoO3−x@PPy at various scan rates, the pseudo-capacitance equation was utilized: i = k1v + k2v1/2. This equation takes into account k1 and k2 as constants, with k1v representing the theoretical value of the pseudo-capacitance contribution. Fig. 5c and S5† showcase the outcomes of this calculation for Zn//MoO3, Zn//MoO3−x, and Zn//MoO3−x@PPy batteries with varying scan rates ranging from 1 to 10 mV s−1. Upon comparison of the pseudocapacitance contribution at a scan rate of 10 mV s−1, it is evident that the Zn//MoO3−x@PPy battery exhibits the highest pseudocapacitance contribution, indicating superior rate performance. This finding corroborates with the data presented in Fig. 4d. Additionally, it is worth noting that the Zn//MoO3−x@PPy battery achieves a significant capacitance contribution of 86% at 10 mV s−1, further highlighting the dominance of pseudocapacitance in determining its performance (Fig. S6†). Notably, this observation is consistent with the outcomes obtained from our experiments and analysis. The MoO3−x@PPy active material possesses a pseudocapacitive nature that facilitates selective storage of Zn2+ ions at the electrode surface. This results in a shortened ion transport distance and an enhanced electron transport rate, ultimately leading to improved rate capabilities and longer cycle life of the electrode material. Zn2+ diffusion coefficients DZn2+ in the MoO3, MoO3−x and MoO3−x@PPy cathodes were also investigated through the galvanostatic intermittent titration technique (GITT). From Fig. 5d and S7,† all three electrodes exhibit a curve shape similar to the GCD curve (Fig. 4b). The ion diffusion coefficient of the MoO3−x@PPy electrode consistently surpasses that of the MoO3 and MoO3−x electrode, indicating that the ion diffusion rate is enhanced by coating it with PPy and low-valence-state Mo introduction (Fig. 5e and S7†). The electrochemical impedance spectroscopy (EIS) data for all electrode materials is presented in Fig. 5f. This figure clearly illustrates that the MoO3−x@PPy electrode exhibits a smaller semicircle in the high frequency region, which indicates a lower charge transfer resistance (Rct). The Rct of MoO3−x@PPy is approximately 278.3 Ω, lower than that of MoO3−x (357.5 Ω) and commercial MoO3 (769.9 Ω), demonstrating that the Rct of the MoO3−x@PPy electrode material can be greatly boosted by the low-valence-state Mo introduction and PPy coating strategies. Furthermore, in the low frequency region, the MoO3−x@PPy electrode demonstrates a steep linear slope, implying efficient electron diffusion capability. This is in contrast to the other electrode materials tested, which exhibit a lower and less steep slope in this region.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3ra02350h |
This journal is © The Royal Society of Chemistry 2023 |