Marzouk Adela,
Ahmed M. A. El Naggar*b,
Ahmed Bakryc,
Maher H. Hilalc,
Adel A. El-Zahhar
d,
Mohamed H. Taha
e and
A. Marey
f
aAluminum Sulphate Company of Egypt, Egypt
bEgyptian Petroleum Research Institute (EPRI), Nasr City, Cairo, Egypt. E-mail: drmeto1979@yahoo.com
cChemistry Departments, Faculty of Science, Helwan University, Cairo, Egypt
dDepartment of Chemistry, Faculty of Science, King Khalid University, Abha 9004, Saudi Arabia
eNuclear Materials Authority, P.O. Box 530, El Maddi, Cairo, Egypt
fDepartment of Basic Science, The Valley Higher Institute for Engineering & Technology, Al-Obour 11828, Egypt
First published on 23rd August 2023
Effluent water from different industries is considered one of the most serious environmental pollutants due to its non-safe disposal. Therefore, proper treatment methods for such wastewater are strongly stimulated for its potential reuse in industries or agriculture. This study introduces a composite fabricated via doping of polystyrene with nanoparticles of cobalt hydroxide as a novel adsorbent for dye and heavy metal decontamination from wastewater. The adsorbent fabrication involves the preparation of polystyrene via high-internal phase emulation (HIPE) polymerization followed by its intercalation with particles of alkali cobalt. The chemical composition and structural properties of the synthesized composite were confirmed by X-ray diffraction (XRD), Fourier transform infrared (FTIR) spectroscopy, and energy-dispersive X-ray spectroscopy (EDX). Moreover, scanning electron microscopy (SEM) and N2 adsorption–desorption surface area analysis were performed to identify the surface and morphological characteristics of the composite. Then, the ability of this structure toward the removal of methylene blue dye (MB) and heavy metal (iron III) species from waste aqueous solutions was investigated. Successful elimination for both MB and Fe(III) was achieved by the presented composite. Elevated adsorption capacities of 75.2 and 112.3 mg g−1, toward MB and Fe(III) respectively, were detected for the presented polymer-metal hydroxide composite. The increased values of the composite are attributed to the presence of both organic and inorganic functional groups within its structure. Kinetic and isotherm studies for the removal of both cationic species revealed that adsorption processes fit the pseudo-second-order kinetic model and Langmuir isotherm model. Additionally, thermodynamics measurements indicated that the adsorption process of methylene blue and Fe ions is feasible, spontaneous, physisorption, and endothermic.
Enormous efforts and several research studies have reported the remediation of water pollution caused by species such as dyes and metal ions. Various techniques including reverse osmosis,10 flocculation,11 electrochemical precipitation,12 ion exchange13 and adsorption14–16 have been developed and utilized to circumvent water pollution. Among these techniques, adsorption has been extensively used to remove metal ions and dyes from wastewater samples since it offers process simplicity, low operating costs and high efficiency.17–21 Efficient adsorbents for such removals may include zeolites, polymers, bio-carbon materials, metal oxides and clays.1–5
Of these structures, polymers are characterized by many good features including tolerability, good mechanical properties and low fabrication costs. Therefore, they are widely employed in many applications such as packaging, tissue engineering, drug delivery and wastewater remediation.22,23 Polymer composites can offer superior properties to individual polymers in some specific applications such as transportation, marine, aerospace/defense, electromagnetic shielding and wastewater treatment.24,25 The adsorption efficiency of polymer composites toward the present pollutants in wastewater samples has been extensively studied over the past few decades.26,27 Among these composites, metal–organic framework/poly-dopamine28 and clay-based composites29 are found to exhibit enhanced absorptivity toward water contaminants. Furthermore, inorganic structures such as metal oxides and hydroxides offer unique physical and chemical properties such as large specific surface areas and abundant active sites. Hence, they have been applied in many applications including catalysis and water treatment.30 However, their high surface-to-volume ratio increases the tendency of their particles to aggregate together. Thus, combining metal oxides or hydroxides with polymers or metal organic framework structures produces hybrid organic/inorganic materials through which the aggregation of particles can be avoided. Additionally, these composites may exhibit properties that are not presented by their composing materials separately.22–24
Polystyrene-activated carbon composites were used effectively for the removal of methyl orange as an organic pollutant from wastewater.31 A novel hybrid nanomaterial was fabricated by encapsulating ZrO2 nanoparticles into spherical polystyrene beads (MPS) covalently bound with charged sulfonate groups (–SO3−) and applied for the removal of Pb(II) from wastewater.32 A polystyrene/AlOOH hybrid material has been prepared by a sol–gel method and applied for Pb(II) decontamination from wastewater.33 Polystyrene/CuO/calcined layered double hydroxide (PS/CuO@CLDH) microspheres were successfully fabricated by the dispersion polymerization method and applied for the efficient removal of Congo red (CR) from wastewater.34 A poly(styrene-block-acrylic acid) di-block copolymer/Fe3O4 magnetic nanocomposite (abbreviated as P(St-b-AAc)/Fe3O4) was prepared by a reversible addition fragmentation transfer (RAFT) method and applied for the removal of antibiotic compounds from wastewater.35 A calcium–barium phosphate (CBP) composite membrane with 25% polystyrene was prepared by a co-precipitation method and utilized for the efficient desalination of saline water and more importantly demineralization process.36 Titanium dioxide nanowires (TiO2-NWs) were successfully prepared by a hydrothermal method and then embraced in polystyrene (PS) to form nanocomposites via emulsion polymerization of styrene monomers in the presence of different ratios of TiO2 nanowires. The prepared polystyrene/TiO2-NW nanocomposite material was applied for the removal of organochlorine pesticide (OCPs) residues from contaminated water.37
In agreement with the trend of wastewater purification via adsorption, this study introduces a composite made up of cobalt hydroxide and polystyrene as a novel structure for the removal of methylene blue dye and iron species from waste aqueous solutions. The novelty of this research work is based on presenting a composite adsorbent for the removal of heavy metals and dyes, with a different composition (PS–Co(OH)2) than those previously reported in the literature, which are generally based on carbon structures, functionalized polymers and metal oxides (or mixed-metal oxides). Moreover, the introduced composite in this study relies on the presence of OH anions to interact with cationic species as well as the presence of cobalt (cation), which can have affinity to anionic species and heavy metals too. Therefore, this composite shows tendency and effective selectivity toward several species simultaneously, unlike other presented adsorbents in previous studies, which mostly have selectivity toward a certain substance. In addition, the presence of OH groups can facilitate extra adsorption mechanisms via hydrogen bonding and anion exchange; thus, several adsorption mechanisms can potentially take place, at the same time, by PS–Co(OH)2. Furthermore, the use of PS with highly porous nature as support to Co nanoparticles could help in their high dispersion, leading to good enhancement for the adsorption performance of the introduced composite in this research work. The adsorption efficiency of this composite, under the effect of different operational parameters, was investigated. Moreover, the kinetics and thermodynamics of the introduced adsorption processes were also studied.
Formula | CAS number | Assay | Supplier | |
---|---|---|---|---|
Industrial wastewater sample (1); contains Fe3+ (100 mg L−1) | N/A | N/A | N/A | Textile companies in El Obour city, Egypt |
Industrial wastewater sample (2); MB dye (40 mg L−1) | N/A | N/A | N/A | Iron foundries in Abu Zaabal, Egypt |
Styrene | C6H5CH![]() |
100-42-5 | ≥99.0% | Sigma-Aldrich Co. (St Louis, MO, USA) |
Potassium per sulfate | K2S2O8 | 7727-21-1 | ≥99.0% | |
Sodium dodecyl sulfate | CH3(CH2)11OSO3Na | 151-21-3 | ≥98.5% | |
Ferric chloride | FeCl3 | 7705-08-0 | 97% | |
Methylene blue dye | C16H18ClN3S·3H2O | 122965-43-9 | N/A |
The concentration of the MB solution was determined using a UV-visible spectrophotometer (Jasco V-550, Japan) at 663 nm based on a calibration curve that was previously constructed through utilizing various solutions of MB with known initial concentrations.8 The concentration of iron in the aqueous solution was determined utilizing the Egyptian Standard method 1700/1989 as follows. Particularly, each tube of measuring included 2.5 mL of hydrochloric acid, which was then supplemented with up to 25 mL distilled water. A drop of KMnO4 was then added to obtain a pink-colored solution. Next, 5 mL KSCN (20%) was added, where the volumes were made up to 50 mL with distilled water. Then, these solutions were measured using a spectrophotometer at a wavelength of 520 nm.38 The sorption efficiency%, sorption capacity qe (mg g−1), and the dimensionless distribution constant (KC) were calculated using the following equations:17
![]() | (1) |
![]() | (2) |
![]() | (3) |
The first peak at 3026 cm−1 was assigned to the aromatic C–H stretching vibration, while the second peak assigned to aliphatic C–H stretching was seen at 2917 cm−1. The next three peaks located at 1596, 1485 and 1451 cm−1 respectively were ascribed to the aromatic C–C stretching vibration. The noted peaks at 1233, 1046, 751, and 695 cm−1 were attributed to the vibrational aromatic C–H deformation. The exhibited functional groups in the tested sample qualitatively confirm the successful synthesis of polystyrene.39
The metal hydroxide particles tended to distribute in a good manner throughout the surface of PS. Furthermore, the provided data through the EDX spectrum (Fig. 3) revealed the detection of both Co and O in the as-prepared composite, which is explained due to the successful incorporation of metal hydroxide particles with polystyrene structures. The quantitative Co weight percent, as given by EDX, was found to be 6.9 wt%, which perfectly agrees with the calculated element weight during the preparation stage. This percentage indicates the existence of proper amounts of Co on the surface of the polymer, which is in agreement with the exhibited morphology of Co(OH)2/PS composites through the SEM image. Simultaneously, a high percentage of the C element was noticed through the elemental analysis that are attributed to the polystyrene structure of quite high molecular weight.
The structural characteristic of the composite was acquired by both FTIR and XRD analyses, as respectively shown in Fig. 4 and 5. With regard to the exhibited FTIR spectrum, absorption bands similar to those formerly noticed for blank polystyrene could be detected for the investigated composite. Nevertheless, the intensities of these peaks could be reduced and their shapes had been slightly deformed. These changes in FTIR absorption bands are attributed to the born strain stress in polystyrene particles due to the loading of Co-hydroxide onto their surfaces. Additionally, the presence of hydroxide particles within the structure of the composite was further verified by observing a new intense broad absorption band centered at 3442 cm−1. This FTIR band could be attributed to the stretching vibration mode of –OH, which is present in cobalt hydroxide.
The results of X-ray diffraction (XRD), performed on the Co(OH)2/PS composite, are shown in Fig. 5. The noticed diffraction peak centered at 2θ = 19.54° corresponded to the non-crystalline regions of the composite due to the amorphous nature of polystyrene. The observed diffraction peaks at 2θ = 32.5°, 38.5° and 58.97° were assigned to Co(OH)2. These signals are quite sharp with low intensities, which referred to the formation of Co(OH)2 in the shape of crystals; however, they are present with limited number in the composite structure. The displayed XRD pattern could confirm the precipitation of metal hydroxide within the polymer geometry.40
The specific surface area of the particles of Co(OH)2/PS composites was determined from the adsorption branch of the N2 adsorption–desorption isotherm using the Brunauer, Emmett and Teller (BET) eqn (4).
![]() | (4) |
Fig. 6 displays the plot of P/[V(P0 − P)] against P/P0, as experimentally collected from the N2 adsorption measurements, where a straight line referring to a correlation coefficient of 0.845 was observed. Thus, the particles of the Co(OH)2/PS composite could exhibit a quite high specific surface area (SBET) value of 186.1 m2 g−1. This result indicates that the Co(OH)2/PS composite can offer extended adsorption capacity, reflecting its high potential for up-taking the different adsorbates from wastewater samples.
Fig. 7-I displays the effect of shaking time (10–300 min) on the MB sorption capacity. The attained data declare that the sorption capacity is positively increased as the reaction time increases up to about 150 min (equilibrium state). This could be attributed to the availability of active function groups on the composite surface.7,8 The maximum sorption capacity was ∼33.5 mg g−1 at equilibrium. By prolonging the equilibrium time, a steady state was observed. This could be explained based on the surface-active function groups' saturation.7,8 Fig. 7-II exhibits the variation in sorption capacity as a function of sorbent dose (0.5–3 g L−1). The obtained results indicated that the increase in the sorbent amount of addition is depicted by ramp down in MB sorption capacity, which could be attributed to that the low dye molecule concentration was not equivalent to the available sorbent surface functional groups.17
The change in sorption capacity with the variation in MB initial concentration (10–100 mg L−1) is shown in Fig. 7-III. The obtained results explore the increment in the sorption capacity as the adsorbate initial concentration increases. This performance could be due to the availability of active functional groups on the Co(OH)2/PS composite surface for binding to dye molecules.20,21
The impact of reaction temperature (25–70 °C) on the MB sorption capacity could be explored from Fig. 7-IV. The exhibited results indicated that the negative influence of the reaction temperature on the sorption capacity reflects the exothermic nature of the MB sorption process.20,21 The same exothermic nature has been recognized for MB sorption from wastewater using arginine modified activated carbon,7 bone char,14 hydroxyapatite sodium alginate,20 and thiosemicarbazide-functionalized graphene oxide composite.21 Fig. 7-V displays the effect of solution pH (2–10) on the MB sorption process. From the Figure, it is clear that the sorption capacity improved as the solution pH increased up to pH 4. The sorption capacity is almost stable at solution pH 4–8. The obtained results are consistent with the literature.7,20 The increase in solution pH has negative effects on the MB sorption process.
The dependence of Fe(III) sorption capacity on reaction time (10–300 min) was investigated, and this is explored in Fig. 8-I. The displayed data demonstrate that the Fe(III) sorption capacity is rapidly increasing as the shaking time increases up to 90 min and then reached the steady state. This means that the sorption equilibrium is achieved at 90 min. The maximum sorption capacity at equilibrium is about 40 mg g−1. The rapid increase in the sorption process before equilibrium state is due to the free surface-active sites on the composite; however, after equilibrium, the steady state is achieved due to the occupation of most of the composite active sites.15,16 Fig. 8-II shows the impact of the composite amount of addition (0.5–4 g L−1) on the Fe(III) sorption capacity. The exhibited results indicated that the sorption capacity is dramatically decreased with the increment in sorbent dose. This performance could be due to that the low dye molecule concentration was not equivalent to the available sorbent surface functional groups.15–17
The impact of Fe(III) ion initial concentration (40–200 mg L−1) on the sorption capacity is illustrated in Fig. 8-III. The displayed results indicated the positive impact of the metal ion initial concentration could be due to the availability of active function groups on the Co(OH)2/PS composite surface for binding to Fe(III) ions.18,19 The variation in Fe(III) ion sorption capacity as a function of reaction temperature (25–70 °C) is explored and presented in Fig. 8-IV. The obtained results indicated that the sorption process is endothermic, whereas the increment in reaction temperature improves the sorption capacity. The same endothermic nature was reported for iron ion sorption from wastewater using chitosan,15,18 silica-supported organic–inorganic hybrids,16 and pecan shell-based activated carbon.19
Fig. 8-V shows the impact of solution pH (2–10) on the Fe(III) ion sorption process. From the figure, it could be observed that the Fe(III) sorption capacity was low in the acidic medium and tended to increase the pH value 12.0. Iron(III) precipitation was observed at pH 6.0 onwards, and the intensity of precipitation increases with the increase in pH from 6.0 to 10.0, which reflects that the removal may be due to the formation of metal hydroxide precipitation.15,16
![]() | (5) |
![]() | (6) |
qt = Kidt0.5 + Ci | (7) |
![]() | (8) |
The plot of the Lagergren model was exhibited as the variation in log(qe − qt) as a function of time (Fig. 9-I), the illustration of time/qt against time (Fig. 9-II) represents the pseudo-second-order model, Fig. 9-III displays the relation between qt and time0.5 (Weber and Morris model), while the Bangham plot is displayed by the double logarithmic plot (Fig. 9-IV). The attained values of the kinetic parameters were declared in Table 2.
![]() | ||
Fig. 9 Illustration of the kinetics of pseudo-first-order (I), pseudo-second-order (II), Weber–Morris (III), and Bangham (IV) models for MB and Fe(III) process. |
MB | Fe(III) | ||
---|---|---|---|
Lagergreen pseudo first-order | k1 (min−1) | 0.016 | 0.012 |
qecal (mg g−1) | 25.4 | 16.6 | |
qeexp (mg g−1) | 35.2 | 44.4 | |
R2 | 0.947 | 0.953 | |
Pseudo second-order | k2 (min−1) | 0.001 | 0.022 |
qecal (mg g−1) | 37.9 | 45.7 | |
qeexp (mg g−1) | 35.2 | 44.4 | |
h (mol g−1 h−1) | 1.52 | 45.66 | |
t1/2 (h) | 24.9 | 1.0 | |
R2 | 0.993 | 0.998 | |
Weber and Morris model | Stage I | ||
ki (mg g−1 min−1/2) | 1.78 | 1.67 | |
C | 11.0 | 23.2 | |
R2 | 0.991 | 0.961 | |
Stage II | |||
ki (mg g−1 min−1/2) | 0.33 | 0.55 | |
C | 29.5 | 34.8 | |
R2 | 0.998 | 0.993 | |
Bangham's equation model | ko (mg g−1 min−1) | 0.05 | 0.06 |
α | 0.67 | 0.37 | |
R2 | 0.957 | 0.957 |
The values of the kinetic parameters (Table 2) indicate that the pseudo-second-order kinetic model possesses the highest coordination coefficient (R2 ≥ 0.99). Besides, the calculated sorption capacities from the pseudo-second order (qecal) for MB and Fe(III) ions (37.9 and 45.7 mg g−1 respectively) are close to the experimental sorption capacity (qeexp) for MB (35.2 mg g−1) and Fe(III) ions (44.4 mg g−1). This means that MB and Fe(III) sorption process using the Co(OH)2/PS composite is fitted well to the pseudo-second order model. This indicates the chemisorption nature for MB and Fe(III) sorption from wastewater, and the removal process involves electron sharing between the composite surface active sites and dye molecules and Fe(III) ions.41–43 The same kinetic profile was reported for methylene blue and Fe(III) sorption from wastewater using iron-based metal organic frameworks,8 hydroxyapatite sodium alginate,20 and thiosemicarbazide-functionalized graphene oxide composites.21 Moreover, Fe(III) removal from wastewater using chitosan,15,18 silica-supported organic–inorganic hybrids,16 and pecan shell-based activated carbon19 was also obeyed to the pseudo-second-order kinetic model.
The tendency of the prepared composite towards MB and Fe(III) ions could be ranked as follows: Fe(III) ions (44.4 mg g−1) > MB molecules (35.2 mg g−1). Furthermore, the values of the half equilibrium time of MB are higher than those of Fe(III) ions (MB: 1.5 h; Fe(III): 45.6 h), while the initial sorption rate for MB (24.9 mol g−1 h−1) is less than that of Fe(III) ions (1.0 mol g−1 h−1). This performance confirms that the composite exhibits a higher tendency toward Fe(III) ions than toward MB molecules, and indicates that the equilibrium state for the Fe(III) ion sorption reaction is faster than that of the MB sorption reaction, which is consistent with the experimental results, whereas the equilibrium state for Fe(III) ions is obtained after 90 min, while the MB equilibrium state is reached after 150 min.
The Weber–Morris kinetic model is applied to explore the mechanism of MB and Fe(III) ion sorption using a Co(OH)2/PS composite. The relation between qt versus time0.5 (Weber and Morris plot) displays the mechanisms that control the sorption process, whether it is a solo or multi-reaction mechanism. The sorption process is controlled by a solo reaction mechanism if the plot exhibits a linear relationship passing through the origin; however, it is controlled with multiple mechanism if the plot consists of several segments.42,43 Fig. 9-III declares that the MB and Fe(III) sorption processes are controlled with multi-reaction mechanisms, whereas the plot consists of two segments. This indicates that the sorption process was performed through two stages; the first stage expresses the sorption process up to reaction equilibrium (150 min for MB and 90 min for Fe(III) ions). This stage was characterized by the rapid rate of reaction, which is due to the availability of free active sites on the composite surface.41,42 The second stage extends after equilibrium time, and was characterized by the slow rate of reaction, which could be attributed to fill most of the adsorbent surface area holes.41–43
It is worth noting that the first stage of Mb and Fe(III) ion sorption processes possess a lower constant C (boundary layer effect) and a higher rate of reaction than the second stage, reflecting that the sorption process in the first stage occurs at the sorbent surface (high rate of reaction), while in the second stage, the sorption process takes place inside the sorbent pores and the intra-particular diffusion is the controlling mechanism (low rate of reaction).17,41–43 The same kinetic profile was reported for methylene blue and Fe(III) sorption from wastewater using iron-based metal organic framework,8 hydroxyapatite sodium alginate,20 thiosemicarbazide-functionalized graphene oxide composite,21 chitosan,15,18 silica-supported organic–inorganic hybrids,16 and pecan shell-based activated carbon,19 which also obeyed the pseudo-second-order kinetic model.
The Bangham kinetic plot (Fig. 9-IV) exhibits a good linear relationship (R2 ≥ 0.95), which reflects that the MB and Fe(III) ion sorption process is also controlled by the diffusion of adsorbate species into the pores of prepared composites.41–43 This result is consistent with the findings by Weber–Morris kinetics, whereas the sorption process is controlled with multiple reaction mechanisms.
![]() | (9) |
![]() | (10) |
ln![]() ![]() | (11) |
![]() | (12) |
The variation in ln qe against lnCe (Fig. 10-I) was applied to verify the Freundlich isotherm model, the Langmuir model plot (Fig. 10-II) relate Ce/qe versus Ce, Fig. 10-III displays the relation between qe and ln
Ce (Temkin isotherm model), while the relation between ln
qe and ε2 (D–R model plot) is shown in Fig. 10-IV. The values of the isotherm model parameters are displayed in Table 3. The anticipated results declare that MB and Fe(III) ion sorption processes obeyed the Langmuir isotherm model, but they possess the highest coordination coefficient (R2 = 0.99). This means that the industrial raffinate effluent treatment using the prepared composite is a homogeneous and monolayer process.42–44 The same isotherm performance was reported for wastewater treatment using iron-based metal–organic frameworks,8 hydroxyapatite sodium alginate,20 thiosemicarbazide-functionalized graphene oxide composites21 for methylene blue sorption process, and chitosan,15,18 silica-supported organic–inorganic hybrids,16 and pecan shell-based activated carbon19 for the Fe(III) removal process.
![]() | ||
Fig. 10 Illustrate of the isotherm of plots of Freundlich (I), Langmuir (II), Temkin (III), and D–R (IV) models for MB and Fe(III) processes. |
MB | Fe(III) | ||
---|---|---|---|
Freundlich isotherm model | N | 2.1 | 1.6 |
KF (mg g−1) | 13.0 | 3.7 | |
R2 | 0.98 | 0.99 | |
Langmuir isotherm model | qm (mg g−1) | 75.2 | 112.3 |
b (L mg−1) | 0.16 | 0.97 | |
R2 | 0.99 | 0.98 | |
R–D isotherm | β (mol2 kJ2) | 0.61 | 0.18 |
qm (mmol g−1) | 9.1 | 11.7 | |
E (kJ mol−1) | 0.9 | 1.7 | |
R2 | 0.76 | 0.86 | |
Temkin isotherm | b (J mol−1) | 173.60 | 99.14 |
B | 14.3 | 25.0 | |
KT (L g−1) | 2.4 | 0.1 | |
R2 | 0.97 | 0.98 |
Table 3 declares that the Co(OH)2/PS composite exhibits higher sorption tendency for Fe(III) ions (qm = 112.3 mg g−1) than for MB molecules (qm = 75.2 mg g−1). The feasibility of MB and Fe(III) sorption processes could be explored from the values of the dimensional constant separation factor (RL), whereas sorption is feasible if 1 〈RL〉 0, while it is an unfavorable process if RL is higher than 1.17,42–44 Fig. 11 shows that the values of RL are between 0.3 〈RL〉 0 for MB, and 0.1 〈RL〉 0 for Fe(III) ions, which indicates that the sorption process using the Co(OH)2/PS composite is a feasible process.
The Freundlich isotherm model exhibits a proper coordination coefficient (R2 = 0.98), which reflects that the multilayer sorption process could be present during the MB and Fe(III) ion sorption process.42–44 In addition, the n values are > 1 (2.05 for MB and 1.65 for Fe(III) ions), indicating the favorable adsorption conditions.17 The Temkin isotherm model possesses a proper coordination coefficient (R2 = 0.98), which indicates that this model could also describe well the obtained experimental results. The Temkin isotherm parameters indicated that the heat adsorption of MB and Fe(III) ions are 173.6 and 99.1 J mol−1 respectively, and the heat adsorption binding constants of the sorption process are 2.4 and 0.1 L g−1 for MB and Fe(III) ions respectively.
The sorption capacity of the applied Co(OH)2/PS composite was compared with other sorbents reported in the literature, and this is shown in Table 4. The applied sorbent shows a relatively fast kinetics, and the equilibrium state is achieved within 240 min. Besides, good removal efficiency at room temperature reflects an energy-efficient process. Finally, the sorption performance and stability of the applied sorbent indicate a promising material for the wastewater treatment approach.
Sorbent type | Ce, mg g−1 | Time, min | Temp, °C | pH | qe, mg g−1 | Ref. |
---|---|---|---|---|---|---|
MB | ||||||
Graphene hybridized polydopamine-kaolin composite | 5–40 | 1440 | 27 | — | 39.6 | 45 |
Bentonite and opuntiaficusindica | 10–360 | 15 | — | 6 | 30.1 | 11 |
Mesoporous CuO@BSS nanocomposite | 5–100 | 30 | — | 10 | 50.0 | 46 |
Magnetic clinoptilolite/chitosan/EDTA | 10–50 | 120 | 40 | 5.5 | 44.4 | 47 |
Silica aerogel/Ni/C/N | 5–100 | 30 | 30 | — | 115.0 | 48 |
Fe3O4@C nanocomposite | 15–40 | 720 | 25 | 7 | 52.5 | 49 |
Fe-BDC MOF | 1–5 | 1440 | — | — | 8.6 | 8 |
Co(OH)2/PS composite | 10–100 | 180 | 25 | 6.5 | 75.2 | P.W. |
![]() |
||||||
Fe(III) ions | ||||||
Silica-supported organic–inorganic hybrid sorbents | 50–700 | 30 | 25 | 5 | 97.1 | 16 |
Pecan shell based activated carbon | 25–100 | 90 | 30 | 3 | 41.6 | 19 |
Cross-linked chitosan | 3–9 | 60 | — | 5 | 64.1 | 18 |
Chitosan | 10–50 | 240 | 30 | 4 | 28.7 | 15 |
Rice husk ash | 2–40 | 60 | 5 | 25 | 6.21 | 50 |
Chitosan/polyethylene glycol blend membrane | 2–10 | 80 | 27 | 5 | 90.9 | 51 |
Activated carbon from coconut shells | 20–100 | 90 | 25 | 6 | 81.8 | 52 |
Co(OH)2/PS composite | 40–200 | 180 | 25 | 2 | 112.3 | P.W. |
![]() | (13) |
−ΔGo = 2.303RT![]() ![]() | (14) |
ΔGo = ΔHo − TΔSo | (15) |
The values of the thermodynamic variables are exhibited in Table 5. The displayed results explore that MB is exothermic in nature, whereas it exhibits a negative ΔH value (−30.6 kJ mol−1). On the contrary, Fe(III) ion sorption is an endothermic process, whereas it possesses a positive ΔH value (14.8 kJ mol−1). The Gibbs free energy change (ΔG) for both MB and Fe(III) ions is negative, which reflects a feasible and spontaneous reaction.41–43 The MB sorption process is characterized by decreasing the randomness at the solid–solution interface, whereas it shows a negative ΔS value (−31.9 kJ mol−1 K); however, the Fe(III) sorption process exhibits a positive ΔS value (110.7 kJ mol−1 K) reflecting an increase in the randomness at the solid–solution interface.41–43 The same thermodynamic performance (exothermic, spontaneous, and feasible process) was reported for methylene blue sorption from wastewater using iron-based metal organic frameworks,8 hydroxyapatite sodium alginate,20 and thiosemicarbazide-functionalized graphene oxide composites.21 Moreover, Fe(III) removal from wastewater by sorption thermodynamics properties such as endothermic, spontaneous, and feasible processes was reported for wastewater treatment using chitosan,15,18 silica-supported organic–inorganic hybrids,16 and pecan shell-based activated carbon.19
ΔG (kJ mol−1) | ΔH | ΔS | |||||
---|---|---|---|---|---|---|---|
25 °C | 40 °C | 50 °C | 60 °C | 70 °C | (kJ mol−1) | (J mol K−1) | |
MB | −21.1 | −21.0 | −20.6 | −20.1 | −19.7 | −30.6 | −31.9 |
Fe(III) | −18.1 | −19.8 | −21.1 | −22.0 | −23.1 | 14.8 | 110.7 |
This journal is © The Royal Society of Chemistry 2023 |