Soyeb
Pathan
*ab,
Menon
Ankitha
c,
Ajith Arjun
Mohan
d,
Neermunda
Shabana
c,
Yongfeng
Tong
e and
P. Abdul
Rasheed
*cd
aResearch and Development Cell (RDC), Parul Institute of Applied Sciences, Parul University, Waghodia, Vadodara, Gujarat 391760, India. E-mail: khan_9751@yahoo.com
bDepartment of Chemistry, Parul Institute of Applied Sciences, Parul University, Waghodia, Vadodara, Gujarat 391760, India
cDepartment of Chemistry, Indian Institute of Technology Palakkad, Palakkad, Kerala 678 557, India
dDepartment of Biological Sciences and Engineering, Indian Institute of Technology Palakkad, Palakkad, Kerala 678 557, India. E-mail: abdulrasheed@iitpkd.ac.in
eQatar Environment and Energy Research Institute, Hamad Bin Khalifa University, P.O. box 5825, Doha, Qatar
First published on 21st November 2023
Graphitic carbon nitride (g-C3N4) and its composites for the hydrogen evolution reaction (HER) have gained immense attention owing to their facile synthesis technique and favorable catalytic performance. Herein we present a composite prepared using a g-C3N4 and H3PW12O40 polyoxometalate (POM) electrocatalyst synthesized by a novel approach for HER application. The electrocatalyst is synthesized by the complexation of a tailored POM, i.e. Ru-substituted polyoxometalate (PW11Ru), with melamine followed by calcination under an inert atmosphere. The proposed monomer complexation strategy utilizing well-defined modulated PW11Ru as a metal precursor provided a unique approach for the preparation of a highly dispersed matrix to form a RuW/g-C3N4 composite. The HER activity of the obtained RuW/g-C3N4 composite is evaluated and compared with individual components of composites by performing several control experiments. RuW/g-C3N4 exhibited improved electrochemical activity towards the HER with an overpotential of approximately 266 mV at 10 mA cm−2 with a Tafel slope of 63 mV dec−1. This new approach using tailored-transition–metal substituted POMs and melamine as the monomer precursors will be expected to contribute to the development of well-defined cluster-embedded 2D-carbon materials with enhanced electrochemical activities.
In this context, polyoxometalates (POMs), which are atomically well-defined polynuclear metal oxide anions extend unparalleled opportunities to synthesize atomically dispersed active metal centers.22–24 Recently, various well-defined composites of POMs have been reported as efficient electrocatalysts25–28 as well as precursors for the hydrogen evolution reaction (HER).29–32 The studies revealed that the presence of POMs assisted in inducing activity in an otherwise inactive counterpart via a synergistic effect. POMs incorporated into a 2D-carbon matrix also exhibited enhanced activity in energy applications as compared to the parent materials.33–36 The high specific surface energy of isolated atoms in the carbon matrix caused easy migration of individual atoms and resulted in agglomerated large clusters. Thus, it would be interesting to attain “further dispersion” of the isolated metal center via the “coordination islands” concept.37,38 This protocol is expected to minimize or prevent agglomeration of isolated atoms by the incorporation of a metal in lacuna of the POMs to form transition-metal substituted polyoxometalates (TMSPOMs) followed by incorporation to C3N4 sites.
Considering these advantages, well-defined bimetallic clusters embedded in carbon catalysts have been developed (Scheme 1(a)) for electrocatalytic applications. Hydrothermal synthesis of a carbon embedded W–Mo heterodimer catalyst, which was derived from TMSPOMs, was synthesized by Zhang and co-workers.39 The synthesized electrocatalyst exhibited Pt-like HER activity with high stability, showing higher activity than analogous Mo–Mo and W–W homodimer catalysts. Wagberg et al. reported electrocatalysts based on carbon-sub-nanometer FeCoW clusters controlled by different TMSPOMs as precursors.40 Furthermore, multi-step synthesis of single-atom Al and O co-doped Mo2N quantum dots on conductive N-doped graphene from the well-defined Anderson-typed POM anion clusters ((NH4)3[AlMo6O24H6]) for hydrogen production in alkaline media has also been reported.41 It is clear that most of the results comprised: (1) the use of a pre-synthesized 2D-carbon matrix for incorporation of either parent POMs or TMSPOMs and (2) hydrothermal synthesis. Furthermore, synthesis using TMSPOMs as precursors for these groups of materials remains unexplored. Thus, there is a need for the simplified synthesis of tailored carbon-materials with the advantage of TMSPOMs derived from well-defined clusters.
Scheme 1 (a) Various protocols for the synthesis of well-defined nanostructures embedded in a carbon matrix and (b) a monomer complexation approach. |
Hence, in view of the scarce but encouraging literature reports on the synthesis and electrocatalytic activities of these materials, the possibility of combining well-defined molecular model systems paves the way to designing new atomically dispersed nanostructures embedded in g-C3N4 electrocatalysts. Here, g-C3N4 incorporated with well-defined RuW clusters through melamine complexation and its atomic-scale modulation of TMSPOM is reported. This is done by synthesizing Ru-substituted phosphotungstate and subsequent calcination under an inert atmosphere (Scheme 1(b)). As far as we are aware, the specified technique has only been used in two publications. The formation of single atoms (arrays) within g-C3N4 frameworks by the simple heat treatment of a complex between commercially available H4SiW12O40 and melamine has been reported by Antonietti's group.42 Recently our group reported g-C3N4 incorporated well-defined clusters of RuW derived from Ru-substituted phosphotungstate.43 Ru was selected for atomic-scale modification of phosphotungstic acid due to its remarkable electrocatalytic activities and relatively low cost compared to Pt (33% less).44–47 Significantly, the RuW/g-C3N4 composite exhibited enhanced electrochemical activity towards the HER in comparison with individual components. The composite showed an overpotential of around 266 mV at 10 mA cm−2 with a Tafel slope of 63 mV dec−1.
Scanning electron microscopy was carried out using a Carl Zeiss Gemini SEM 300. The image of the synthesized g-C3N4 (Fig. 2(a)) shows stacked 2D sheets with non-uniform pores. The SEM of PW11Ru–Mel (Fig. 2(b)) displays the typical bulk morphology without any structural characteristics. Interestingly, the composite (RuW/g-C3N4) formed by the calcination of melamine in the presence of PW11Ru, i.e. calcination of compound (PW11Ru–Mel) synthesized using the monomer complexation approach, exhibits a “poly dispersed spherical” morphology (Fig. 2(c)) as compared to its counterparts. However, evaluation of the SEM images of the composite (Fig. 2(d)) revealed the presence of folded 2D sheets of RuW/g-C3N4. Thus, it is predicted that due to high wt% of PW11Ru, the RuW-clusters incorporated 2D-sheets agglomerated together to form an overall non-uniform spherical morphology.
Fig. 2 SEM images of (a) g-C3N4, (b) PW11Ru-Mel, and (c) RuW/g-C3N4; (d) magnified image of RuW/g-C3N4. |
The spherical morphology for the bulk RuW/g-C3N4 was further confirmed by transmission electron microscopy (TEM: Tecnai G2, F30) and it is given in Fig. 3(a)–(d), which shows the polydispersed spherical microparticles. Besides, the periphery of dense microstructures shows spicules. For finer extrapolation of the nanostructure of the composites, the material was subject to ultrasonication for an extended period of 30–40 min before TEM imaging.
The interplanar distance was measured for the composites (Fig. 3(c)) and found to be 0.34 nm corresponding to the (002) plane of g-C3N4.52 At higher magnification (Fig. 3(d)), well-dispersed nano-clusters (<2 nm) of RuW(-oxides) throughout the g-C3N4 matrix were observed. This was evident by the elemental mapping of the composite material (Fig. 3), which confirmed the uniform dispersion of elements throughout the g-C3N4 matrix. Moreover, no evidence could be observed for the formation of large metal(s) clusters even in the presence of higher W loading. Thus, the described method of complexation is a promising method for the synthesis of well-dispersed metal-centers.
The XRD diffractogram of g-C3N4, PW11Ru–Mel, and RuW/g-C3N4 is presented in Fig. 4. For g-C3N4, the typical peaks at 12.8° and 27.4° correspond to (100) and (002) planes was observed. These peaks can be ascribed to the layered structure of the tri-s-triazine units53 and the interlayer stacking of the aromatic system.53,54 The presence of a Keggin unit in PW11Ru–Mel was confirmed by the sharp peaks in the region 6° and 9° as well as broad peaks in the 25–30° region.43
The broadness of the peak suggests the loss of crystallinity of the Keggin structure after the complexation between PW11Ru and the melamine monomer. On calcination of PW11Ru–Mel, the formed RuW/g-C3N4 was expected to exhibit a decrease in the number of peaks due to the partial breakdown of the Keggin unit to the corresponding oxide. Thus, RuW/g-C3N4 showed a single broad peak in the region 4°–10°. Moreover, the presence of a broad peak with maxima at around 26° confirmed the presence of the g-C3N4 matrix in the RuW/g-C3N4. Furthermore, no additional peaks of PW11Ru are observed in the region 20–35° and this could be due to the decomposition of the Keggin unit as well as higher dispersion of the corresponding oxides in the g-C3N4 matrix.
XPS measurement was conducted on a Kratos Axis Ultra platform with an Alkα X-ray source of 1486.6 eV and a total energy resolution of around 0.1 eV. The measurement is conducted under a UHV of 10–10 mbar at room temperature. A hemisphere analyser with a take-off angle of 90° to the surface is utilized for signal acquisition. The high-resolution (HR) spectra are measured with a step size of 0.1 eV and a pass energy of 10 eV and the wide scan is with a step size of 1 eV and a pass energy of 100 eV. All binding energy positions are calibrated to the C 1s at 284.8 eV (C–C). The XPS survey spectrum of RuW/g-C3N4 is shown in Fig. S1 (ESI†) and it indicates the presence of C, N, O, Ru, and W, which is an indication of the presence of g-C3N4 and PW11Ru in the composite.55,56
Fig. 5 shows the high-resolution (HR) spectra of C 1s, Ru 3d, W 4f and O 1s with deconvolution GL(30) after a proper Shirley background subtraction. Fig. 5(a) shows the C 1s, in which a proper fitting gives 4 related peaks corresponding to the C–C at 284.8 eV, C–O at 286.5 eV, and two N related signals at 287.0 eV (C–N) and 288.5 eV (N–CN), respectively.57–59Fig. 5(b) presents the Ru 3d with the Ru 3d5/2 located at 280.9 eV and 282.3 eV for Ru4+ (solid-red-line) and Ru5+ (dash-blue-line), respectively.60–62 The related Ru 3d3/2 are given at 284.9 eV (to 280.9 eV) and 286.4 eV (to 282.3 eV) with a spin-orbital splitting of 4.2 eV (for simplicity the C 1s component was hidden). Fig. 5(c) exhibits the W6+ valence state with the W 4f7/2 located at 35.6 eV, which corresponds to the W–O bond.63,64 A blue doublet with W 4f7/2 at 32.9 eV and a green doublet at 33.9 eV can be assigned to the W4+ and W5+ states, which can probably be assigned to the W–C bond.29,64 A loss feature at the higher BE side of 41.4 eV is also observed, which is a signature of the W6+ states.65–69 This again confirms the presence of WO3 in the composites. The corresponding O 1s signal is given in Fig. 5(d), where the different oxidation components, including the W–O/Ru–O at 530.4 eV, the metal hydroxide (M–OH) at 531.8 eV, the carbon related C–O at 533.1 eV and the carbonate (O–CO) at 534.2 eV, can be distinguished.70 The O 1s indicates the possible RuxW(OH)y species in the composites.
Fig. 5 The core level spectra of (a) C 1s, (b) Ru 3d, (c) O 1s and (d) W 4f of the RuW/g-C3N4 composite. |
Inductively coupled plasma (ICP) analysis was carried out to evaluate the concentration of Ru and W in the RuW/g-C3N4 composite and it was found that the percentage of Ru is only 3.7 and the concentration of W is around 59.5% (Table S1, ESI†). This shows that the presence of Ru in the final composite is much less. In addition, we have made Ru/g-C3N4 and W/g-C3N4 composites with the ratio of 3.7 and 59.5% of Ru and W respectively by simply mixing g-C3N4 with salts of Ru and W to compare the HER performances.
The HER activities of the RuW/g-C3N4 samples were studied in 0.5 M H2SO4 solution with a specific amount of sample loaded on a GCE and compared with a bare GCE and Pt/C. As shown in Fig. 6(a), the GCE showed very weak electrocatalytic activity while the Pt/C showed the best HER activity. The onset overpotential of Pt/C is approximately 7 mV, and the overpotential is 69 mV (at 10 mA cm−2). The overpotential of PW11Ru was 446 mV while the corresponding value of g-C3N4 is 427 mV. However, the overpotential of the RuW/g-C3N4 composite was 266 mV, which is around 40% lower than the HER overpotential of g-C3N4 and around 37% lower than the HER overpotential of PW11Ru. These results showed that the HER performance of the RuW/g-C3N4 composite is significantly better compared to its individual components. In addition, at the same overpotential of 266 mV, the current density of RuW/g-C3N4 is 10 mA cm−2, which is higher than that of PW11Ru (2.7 mA cm−2) and g-C3N4 (3.69 mA cm−2) (Fig. S3, ESI†).
Fig. 6 (a) HER polarization curve and (b) the corresponding Tafel plots of PW11Ru, g-C3N4, and RuW/g-C3N4 composites in comparison with Pt/C. |
The Tafel slopes of PW11Ru, g-C3N4, and the RuW/g-C3N4 composite are given in Fig. 6(b) by fitting the linear portion of the polarization curves. The Tafel slope for Pt/C (32 mV dec−1) is lower than all samples for commercial Pt/C. The Tafel slopes for PW11Ru and g-C3N4 are 119 mV dec−1 and 108 mV dec−1, respectively. The Tafel slope for the composite is 63 mV dec−1, which is much lower than that of pure g-C3N4 and PW11Ru and it confirms that the incorporation of PW11Ru on g-C3N4 can significantly enhance the electrocatalyst performance. Here, the enhanced HER performance of RuW/g-C3N4 arises due to the Ru metal centers embedded on the g-C3N4 backbone, which can enhance the HER performance. A comparison table showing the HER performance of POM/g-C3N4-based catalysts is presented in Table 1. The HER performance of the RuW/g-C3N4 composite is comparable with the reported Ru-based POM materials, with a Tafel slope of 63 mV dec−1 even with a lower content of Ru (only 3.7%).
Material | Overpotential@10 mA cm−2 (mV) | (Tafel slope) (mV dec−1) | Ref. |
---|---|---|---|
Co-WS2/P-WO2.9 | 146 and 120 (acidic and alkaline) | 86 and 74 (acidic and alkaline) | 75 |
{Cu2(3-bptzp)3(H2O)4[SiW12O40]}H2O (Keggin-type) | 59.4 (alkaline media) | 74 (alkaline media) | 76 |
Co2P/WC@NC/CNTs | 171 and 198, (0.5 M H2SO4, 1.0 M KOH), | 65 and 42 (acidic and alkaline) | 77 |
[PW11MO39]5-@Ru-rGO | −0.41 and −1.65 (vs. Ag/AgCl) (acidic and alkaline) | 36.56, 107.95 (acidic and alkaline) | 78 |
POM derived Co/WN | 143 (both acidic and alkaline media) | 90 and 118 (acidic and alkaline) | 79 |
Ru-MoO2@PC | 230 (alkaline) | 86.6 (alkaline) | 80 |
Ru doped WO3 | 124 (acid) | 28, 17.6, and 83 (acidic, alkaline, and neutral) | 81 |
2D [Co2(TIB)2(PMo12O40)]·Cl·4H2O | 137 mV (acidic) | 59 (acidic) | 82 |
CoW12/clicked g-C3N4 | 230 | 67 | 83 |
g-C3N4-boron nitride and chitosan | 520 (acidic) | 150 (acidic) | 84 |
RuW/g-C3N4 | 266 (acidic) | 63 (acidic) | This work |
As control experiments, the HER performances of the Ru/g-C3N4 and W/g-C3N4 composites were compared with RuW/g-C3N4 and the results are given in Fig. S4 (ESI†). As shown in Fig. S4 (ESI†), the HER activity of these composites is much less compared to RuW/g-C3N4. It shows that there is appropriate synergy between the precursor and g-C3N4 matrix during the monomer complexation approach, while it is not observed in Ru/g-C3N4 and W/g-C3N4 composites. The control experiments confirm the improved activity as compared to their counterparts, i.e. Ru/g-C3N4, suggesting synergy between Ru and W in RuW/g-C3N4 catalyzed HER. Thus, Ru and W both are predicted as active sites and the electronic interactions between these two metals can catalyze the hydrogen evolution.71 In addition, the presence of WO3 can transfer free electrons to Ru, which results in an interfacial electric field and this electron-rich region on the Ru surface can enhance the binding capability with protons.72,73 Moreover, WO3 in an acidic environment can form a hydrogen tungsten bronze compound (HyWO3) through H insert/insert out, which results in hydrogen transfer from the active site to the WO3 substrate.73,74
To evaluate the interactions between PW11Ru and the g-C3N4 matrix quantitatively, charge-transfer resistance (Rct) and electrochemical active surface area (ECSA) were utilized. Fig. 7(a) shows the CVs of RuW/g-C3N4 at different scan rates and it shows that the current density increases with scan rate. The slope of the current density at −0.15 V and scan rate (Fig. 7(b)) provides double-layer capacitance (Cdl), which can be used as proportional to ECSA. The Cdl of RuW/g-C3N4 was calculated as 14.7 mF cm−2, which was 1.56 times that of g-C3N4 (9.36 mF cm−2), and 2 times that of PW11Ru (7.26 mF cm−2). This increase in Cdl value confirms the enhanced electrical conductivity of the composite due to the incorporation of metal centers into the g-C3N4 matrix.
The Rct values were measured from electrochemical impedance measurements. Fig. 7(c) depicts the typical Nyquist plots of PW11Ru, g-C3N4, and the RuW/g-C3N4 composite, and the Rct value was assessed (inset of Fig. 7(c)). The Rct values are lower for the RuW/g-C3N4 (145 Ω) composite in comparison with PW11Ru (258 Ω) and g-C3N4 (190 Ω) and this corresponds to enhanced electron transfer kinetics of the composite, which is corroborated by the CV data. In addition, the stability of the catalysts is also evaluated, which is an important parameter when considering practical applications. The polarization curve showed a negligible difference of 12 mV after 500 scan cycles in the onset potential (Fig. 7(d)). This negligible difference in the overpotential confirms the long-term stability of the catalyst even in the absence of a binder molecule.
The present work aimed to simplify the preparation of bimetallic-supported C3N4 from tailored POM. Due to the known remarkable electrocatalytic activities of Ru, we have decided to use Ru for the substitution of one of the W from phosphotungstate. We believe that a simplified approach will be useful for developing similar bimetallic catalytic systems with different transition metals. This protocol has numerous advantages, such as straight forward synthetic route, the privilege of module metallic compositions as POMs can be designed at the molecular level, low-cost reagents, non-hydrothermal conditions, and no use of organic templates (in the case of MOF-derived nanoclusters).
Footnote |
† Electronic supplementary information (ESI) available: XPS survey spectra, cyclic voltammogram, current density data, ICP analysis and HER polarization curve. See DOI: https://doi.org/10.1039/d3ma01010d |
This journal is © The Royal Society of Chemistry 2024 |