Patrick H.
Maag
abcd,
Florian
Feist
d,
Hendrik
Frisch
*ab,
Peter W.
Roesky
*c and
Christopher
Barner-Kowollik
*abd
aSchool of Chemistry and Physics, Queensland University of Technology (QUT), 2 George Street, QLD 4000 Brisbane, Australia
bCentre for Materials Science, Queensland University of Technology (QUT), 2 George Street, QLD 4000 Brisbane, Australia. E-mail: h.frisch@qut.edu.au; christopher.barnerkowollik@qut.edu.au
cInstitute of Inorganic Chemistry, Karlsruhe Institute of Technology (KIT), Engesserstraße 15, 76131 Karlsruhe, Germany. E-mail: roesky@kit.edu
dInstitute of Nanotechnology (INT), Karlsruhe Institute of Technology (KIT), Hermann-von-Helmholtz-Platz 1, 76344 Eggenstein-Leopoldshafen, Germany. E-mail: christopher.barner-kowollik@kit.edu
First published on 28th February 2024
Single chain nanoparticles (SCNPs) are a highly versatile polymer architecture consisting of single polymer chains that are intramolecularly crosslinked. Currently, SCNPs are discussed as powerful macromolecular architectures for catalysis, delivery and sensors. Herein, we introduce a methodology based on Förster Resonance Energy Transfer (FRET) to evidence the folding of single polymer chains into SCNPs via fluorescence readout. We initially introduce a molecular FRET pair based on a bimane and nitrobenzoxadiazole (NBD) moiety and study its fluorescence properties in different solvents. We subsequently construct a low dispersity polymer chain carrying NBD units, while exploiting the bimane units for intramolecular chain collapse. Upon chain collapse and SCNP formation – thus bringing bimane and NBD units into close proximity – the SCNPs report their folded state by a strong and unambiguous FRET fluorescence signal. The herein introduced reporting of the folding state of SCNPs solely relies on an optical readout, opening avenues to monitoring SCNP folding without recourse to complex analytical methodologies.
To utilize FRET to probe SCNP folding, we introduce a new FRET pair, based on the fluorophores bimane and nitrobenzoxadiazole (NBD), combining these into initially one molecule which we carefully assess in a preliminary study (1, refer to Scheme 1A). The choice of bimane unit is driven by its fluorescent properties and commercial availability as difunctionalized dibromobimane (2), able to introduce symmetrical cross-links into the polymer chain. Importantly, the fluorescence of the halogenated bimane species is effectively quenched, making them particularly suitable for use as fluorescent labelling agents.33–35 The choice of NBD as counter FRET entity is guided by requiring a moiety that features a comparable fluorescence intensity and shifted emission spectrum compared to the bimane species. We initially demonstrate that the molecular FRET pair 1 functions in organic solvents, specifically tetrahydrofuran (THF), yet shows no FRET activity in aqueous solution. Subsequently, we prepare a water-soluble polymer chain featuring NBD units along its lateral chain as well as carboxylic acid functionalities, which serve as intramolecular crosslinking points. Initiated by dibromobimane 2, the polymer chain is folded into SCNPs, bringing bimane units and NBD together (refer to Scheme 1B). The close proximity and free orientation within SCNPs allow the FRET pair to self-report the folding status by virtue in a variety of solvents, specifically in water. We submit that reading SCNPs' folding status via optical means is a unique methodology to not only gain information about their morphological state, but to follow it during, e.g., catalytic applications.
Molecules with a bimane substructure such as dihydroxybimane (3) or the corresponding diacetate (refer to ESI, Section 3.1.2, Fig. S14†) feature fluorescence spectra with a peak emission of 450 nm and an excitation maximum at 380 nm in THF. The fluorescence spectra of molecules with NBD substructure such as (7-nitrobenzo[c][1,2,5]oxadiazol-4-yl)glycine (4) are similar to the bimane, yet red-shifted by 80 nm (Fig. 1A). Compound 4 displays a peak emission at 530 nm and the excitation maximum at 460 nm in THF. The local excitation minimum of 4 overlaps with the excitation maximum of 3 and therefore allows for the selective excitation of 3 at 380 nm (Fig. 1A). Of key importance is the spectral overlap of the donor emission with the acceptor absorbance spectrum.36 In the present case, the overlap with the acceptor excitation spectrum is identical with the absorbance spectrum (refer to the ESI, Section 3.1.2, Fig. S12†). Compound 1 shows the expected shift in the emission spectrum towards longer wavelengths due to the energy transfer from the donor (bimane) to the acceptor (NBD). Furthermore, the excitation spectrum for an emission of 520 nm combines the excitation spectra of the bimane and the NBD (Fig. 1B). FRET can also be visualized by recording 3D fluorescence spectra of the individual fluorophores and the molecular FRET pair (1). 3 and 4 show their characteristic emission spectrum depending on the excitation wavelength displayed in a heat map (Fig. 1C and D). Combining these into one molecule allows the excitation of both fluorophores and enables the energy transfer to the acceptor, returning the emission spectrum of the NBD (Fig. 1E). The energy transfer can be observed as shift in the intensity to higher emission wavelength.
Fluorescence spectra of 1, 3 and 4 were recorded in THF demonstrate an efficient energy transfer, indicating close proximity and free orientation of both fluorophores. FRET was also observed in DCM, yet was less efficient in acetonitrile and methanol. No FRET was observed in polar solvents as DMF, dimethyl sulfoxide and water (refer to ESI, Section 3, Fig. S5†). The solvent dependent FRET of 1 may be associated with varying orientations of the fluorophores in different solvents. The orientation of emission transition dipole of the donor in comparison to the absorption dipole of the acceptor is an important parameter affecting the Förster distance. The orientation parameter (κ2) can theoretically range from 0 to 4. However, for a freely rotatable system a value of 2/3 is expected.36 Furthermore, earlier studies revealed that solvents effect the rate coefficient of intramolecular FRET and therefore change the efficiency of the energy transfer.37 In the case of 1, the solvent might hinder the free orientation of the donor and acceptor or decrease the efficiency based on a change in transfer rate coefficient, yet may also lead to aggregation-induced quenching. Further investigation of this particular FRET pair would require time-resolved spectroscopy.
The FRET efficiency was determined by photobleaching of the acceptor, comparing the emission of the bimane before and after bleaching (Fig. 2). Therefore, 1 was irradiated for 13 h with λmax = 505 nm until no emissions of the NBD were observed anymore, resulting in an increasing intensity of the bimane emission of 80%. The FRET efficiency is therefore assumed to be close to 80% (refer to the ESI, Section 3.1.2, Fig. S17†). An alternative method to demonstrate the FRET efficiency involves the cleavage of bimane from the NBD. The bimane ester cleavage photoreaction at long irradiation times was studied by Chaudhuri et al.38 Therefore, 1 was irradiated for 25 min with λmax = 415 nm in water resulting in the formation of a carboxylic acid and an alcohol (Fig. 2A and B). The 3D fluorescence spectrum shows the characteristic pattern of both individual fluorophores, indicating that the bond between the donor–acceptor pair is cleaved.
To functionalise P1 with a FRET acceptor, P1 was post-functionalized with N-(3-bromopropyl)-7-nitrobenzo[c][1,2,5] oxadiazol-4-amine (5) by an esterification reaction of the carboxylic acid pendant groups in a solution of THF and caesium carbonate as base (P2, Mn = 47.3 103 g mol−1) (Fig. 3A). During esterification with 5, the hydrodynamic volume of the polymer slightly increases, resulting in an increase of the apparent Mn by 11% (refer to SEC, Fig. 3B) and a slight shift of the P2 SEC elution time compared to the P1. The post-functionalization was closely monitored by comparing the UV/Vis absorption of the polymer in the SEC trace to the refractive index detection (RID). An observed increase in absorption at 450 nm over time evidences the successful incorporation of NBD units within the polymer chain. In a subsequent step, P2 was folded into SCNPs by esterification with dibromobimane 2 in a highly diluted reaction mixture of 0.2 mg mL−1P2 in THF (SCNP1, Mn = 35.7 103 g mol−1, Fig. 3D). During folding, the hydrodynamic volume of the polymer decreases, leading to a 25% reduction in the apparent molecular weight (refer to SEC, Fig. 3B), resulting from a shift of the SCNP1 SEC elution time compared to the P2. Moreover, the UV/Vis absorption of the polymer in the SEC trace at 380 nm increases over time, evidencing the successful incorporation of bimane units within the polymer chain, correlating with the decrease in apparent molecular weight and demonstrating that the bimanes act as cross-links. After 2 h of folding, the incorporation rate decreases, reflected by a stagnation of the absorption at 380 nm in the SEC trace, indicating a saturation of the carboxylic acid pendant group.
To investigate if the observed SCNP formation can be monitored through FRET, a 3D fluorescence spectrum of SCNP1 in water was recorded. Pleasingly, it shows a similar pattern as of the directly linked donor–acceptor pair 1 in THF, indicating an efficient FRET between bimane and NBD moieties within the SCNP architecture resulting from a close proximity of crosslink (donor) and the polymer-bound dye (acceptor). To confirm that the observed 3D fluorescence spectrum is the result of FRET, bleaching experiments were carried out (refer to ESI, Section 3.1.4, Fig. S25 and S26†). The efficient energy transfer between the two fluorophores indicates the folded state, which results from their close proximity and the presence of bimane cross-links, whose fluorescence is initially quenched by bromine functions. Herein, we successfully incorporate both fluorophores within SCNPs, paving the way for further quantitative studies to determine the degree of compaction through an optical readout. The presence of FRET in SCNPs in water also supports the notion of a different orientation parameter in different solvents compared to molecule 1 as described above.
Nevertheless, to study the effect of different degrees of NBD incorporation on the FRET efficiency, SCNPs with different amounts of NBD moieties in their polymer backbone were synthesized and 3D fluorescence spectra were recorded. P1 was post-functionalized with different amounts of NBD moieties (5) utilizing the carboxylic acid pendant groups resulting in P3 (Mn = 42.6 103 g mol−1) and P4 (Mn = 41.6 103 g mol−1) with a slightly increased apparent Mn (Fig. 4). The post-functionalization of NBD units was monitored by UV/Vis absorption at 450 nm of the polymer in the SEC trace showing a decreasing incorporation of NBD moities from P2 to P4. In a subsequent step P3 and P4 were cross-linked with identical amounts of 2 in a highly diluted reaction mixture of 0.2 mg mL−1 in THF resulting in SCNP2 (Mn = 36.1 103 g mol−1) and SCNP3 (Mn = 38.6 103 g mol−1). During folding, the hydrodynamic volume of the polymer decreases, leading to a reduction in the apparent molecular weight, resulting from a shift of the SCNP's SEC elution time compared to P3 or P4. With decreasing amount of NBD moieties, it can be observed that the FRET efficiency decreases, observing no FRET in SCNP3. The difference in emission can be visually observed by irradiating with λmax = 380 nm LED (Fig. 4G).
Further, the photochemical behaviour of SCNP1 and SCNP2 was studied. To demonstrate the efficiency of the FRET, SCNP1 was irradiated for 8 h with λmax = 505 nm until no emission of the NBD was observed, resulting in an increasing intensity of the bimane emission (Fig. 5). We observed that the Mn only changes slightly. Additionally, we irradiated the SCNP2 for 3 h with λmax = 415 nm in water resulting in a decrease of absorption at 380 nm and 450 nm, but also an increase of apparent molecular weight, suggesting that the SCNPs were unfolded to a linear chain. Irradiating the bimane cross-links within the SCNPs leads to a cleavage of the ester bonds, releasing dihydroxybimane 3 and the original polymer with carboxylic acid pendent groups. The unfolding leads to an increase in the hydrodynamic volume, which concomitantly results in an increase in the apparent molecular weight, which is evidenced by a shift of the irradiated SCNPs SEC elution time compared to the SCNP1 (red arrow, Fig. 5E). The shift of the unfolding in the SEC trace appears not as pronounced as the initial folding, which might be due to a small number of remaining bimane cross-links along the chain or side reactions occurring during the photocleavage and bleaching of NBD moieties. Importantly, such a photochemical unfolding of the SCNP was not observed during the fluorescence measurements, which is perquisite to utilise FRET to probe the SNCP architecture.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3sc06651g |
This journal is © The Royal Society of Chemistry 2024 |