Xiangyang Chena,
Xinmei Zhangc,
Jipeng Chena,
Weibin Baiad,
Xiaoxiao Zhengb,
Qi Linb,
Fengcai Lin*b and
Yanlian Xu*b
aCollege of Chemistry and Materials, Fujian Normal University, Fuzhou, 350007, PR China
bFujian Engineering and Research Center of New Chinese Lacquer Materials, College of Materials and Chemical Engineering, Minjiang University, Fuzhou 350108, China. E-mail: linfengcai8@163.com; ylxu@mju.edu.cn
cCollege of Materials Science and Engineering, Huaqiao University, Xiamen 361021, China
dFujian Key Laboratory of Polymer Materials, Fujian Normal University, Fuzhou, 350007, PR China
First published on 7th April 2022
The economic loss and environmental damage caused by metal corrosion is irreversible. Thus, effective methods, such as coating technologies are used to protect metal surfaces from corrosion. In this work, cardanol-based benzoxazine (CB) was synthesized by a solvent-free method using cardanol, paraformaldehyde and n-octylamine. A cardanol-based benzoxazine copper polymer (CBCP) with good mechanical properties was then prepared by CuCl2 catalysis and can be cured at room temperature. Subsequently, polyimide corrosion inhibitors with a two-dimensional sheet structure (pyromellitic dianhydride polyimide (PDPI) and 1,4,5,8-naphthalene tetracarboxylic dianhydride polyimide (NDPI)) were designed and prepared. Lastly, PDPI or NDPI was mixed with CBCP to obtain two-dimensional lamellar polyimide/cardanol-based benzoxazine copper polymer composite coatings. The Tafel curves and electrochemical impedance spectroscopy (EIS) measurements showed composite coatings with good corrosion resistance in different corrosive media. Compared to CBCP coating, the anticorrosion performance of the composite coatings improved obviously, especially the coating obtained with 0.5 wt% PDPI. It exhibits a high polarization resistance (3.874 × 109 Ω), a high protection efficiency (99.99% and 97.98%) and low corrosion rate (3.376 × 10−6 mm year−1). This work suggested a facile and eco-friendly strategy for preparing bio-based anticorrosive composite coatings from low cost and abundant cardanol and polyimide corrosion inhibitors, which will significantly promote their application in metal anticorrosion.
Polybenzoxazine resin has become increasingly popular in anti-corrosion composite coatings because of its close to zero shrinkage, low water absorption, high thermal stability, flexible molecular designability, good dielectric characteristics, and superior mechanical properties.4–6 For instance, Xin et al. synthesized a silane-functional polybenzoxazine coating with good anti-corrosion shielding performance.7 The charge transfer resistance (Rct) of hydrophobic benzoxazine-cured epoxy coating was about 3 fold higher than that of bare steel.8 Compared to the traditional petroleum-based materials, the development and utilization of bio-based materials have become gradually well-liked owing to their easy processing and renewable characteristics.9–11 Such as cellulose,12 cardanol,13 alginate,14 soybean oil,15 and so on. Cardanol, as a natural phenol with abundant yield and easy extraction, was often used in the preparation of anti-corrosion coatings.16 Vijayan et al. synthesized a colorless, transparent, hydrophobic and corrosion resistant coating with cardanol.17 Aggarwal et al. developed an epoxy–cardanol resin using cardanol exhibits better properties as compared to epoxy resin in terms of increase in tensile strength, elongation.18 There are also many reports about cardanol-based benzoxazines. Patil et al. synthesized a bio-based amine functional benzoxazine resin from cardanol shown good mechanical, chemical, and solvent resistance properties.19 Huang et al. combined cardanol-based polybenzoxazine and amino-modified silica nanoparticles to develop a superhydrophobic coating on mild steel for anti-corrosion coating application.20 Hence, cardanol-based benzoxazines with low cost, eco-friendly and excellent mechanical properties are usually prepared from cardanol as a raw material and as a good anti-corrosion matrix material. Nevertheless, the high curing temperature (>200 °C) of benzoxazine limits its application in practical construction process. Therefore, in this work, CuCl2 was used to catalyze the ring-opening reaction of cardanol-based benzoxazine and can be cured at room temperature.
On the other hand, the existence of cracks and holes, as well as the inherent permeability of corroded media and degradation of traditional material matrices during curing shrinkage may significantly reduce the barrier efficiencies of coatings.21 The two-dimensional lamellar materials, such as graphene and its derivatives, boron nitride and molybdenum disulfide, often used as a corrosion inhibitor in anticorrosive coatings due to their unique lamellar structures and high specific surface areas.22–24 Because of special lamellar structure, two-dimensional materials can increase the tortuous diffusion pathways avoiding corrosion mediums directly accessing the substrate surface, leading a good anti-corrosion property.25 However, since most common corrosion inhibitors were composed of inorganic materials, the poor dispersion in organic coatings may also decline the shielding performance of coatings.26 Polyimide was widely used in the field of aeronautics and astronautics, separation membrane and anticorrosive coatings because of its excellent mechanical energy, electrical insulation, thermal stability and chemical resistance.27–29 Therefore, adding two-dimensional lamellar polyimide into resin as a corrosion inhibitor is expected to show significantly effect and further improve the anticorrosion performance of matrix material.
In this work, cardanol-based benzoxazine (CB) was prepared by solvent-free synthesis method using cardanol as raw material. CuCl2 was then introduced into catalyze ring-opening polymerization to form cardanol-based benzoxazine copper polymer (CBCP) that can be cured at room temperature yield excellent mechanical properties. Meanwhile, two aromatic polyimides (PDPI and NDPI) with two-dimensional lamellar structures were designed and prepared, and then added into CBCP as corrosion inhibitors. The results show that the synergistic effect induced between two-dimensional lamellar polyimide with highly insulating and CBCP with excellent mechanical properties yielded, two-dimensional lamellar polyimide/cardanol-based benzoxazine copper polymer composite coatings with excellent anti-corrosive properties.
To further confirm the structure of CB, 1H-NMR analyses of cardanol and CB were performed. As shown in Fig. 2, the peak ranging from 6.60 to 7.10 ppm was attributed to hydrogen atoms present on benzene ring of cardanol, while the solvent peak of CDCl3 was recorded at 7.28 ppm. The displacement peaks at 0.89–2.84 ppm and 4.89–5.87 ppm were attributed to the saturated fat chain and hydrogen atoms on the unsaturated double bond of cardanol, respectively. Obviously, singlet state proton characteristic peaks appeared at 4.86 ppm and 3.97 ppm, corresponding to O–CH2–N and Ar–CH2–N in benzoxazine ring, respectively.31,32 These results further confirmed the successful synthesis of CB.
Heat curing was commonly used in benzoxazine. Where ring-opening polymerization may occur at high temperatures above 180 °C. However, such high reaction temperatures were not suitable for practical applications. In this paper, the CuCl2 catalyzed ring-opening polymerization method was used to prepare CBCP. This route significantly reduced the ring-opening temperature. The FT-IR spectra of CB and CBCP in Fig. 1 showed vanishing characteristic peaks of benzoxazine at 960 cm−1 and 1360 cm−1 after CuCl2 catalytic polymerization. The symmetric and asymmetric stretching vibration peaks of C–N–C at 1035 cm−1 and 1245 cm−1, as well as the asymmetric stretching vibration peaks of C–N–C at 1124 cm−1 also disappeared.33 Thus, the CB monomer underwent ring-opening polymerization, and CuCl2 successfully catalyzed the ring-opening reaction of CB.
Fig. 3 shows the solid-state CP/MAS 13C-NMR spectra of CBCP. As shown in Fig. 3, the peaks at 66.44 and 63.81 ppm correspond to the resonances of methylene carbons (C1 and C2) of O–CH2–N and Ar–CH2–N, respectively.34 Some chemical shifts (ppm) were assigned as follows: 40.13 (C3), 149.76 (C4), 30.19 (C10), and the other resonances of C11, C12, C13, C14, C15, C16, C17 and carbon on the side chain of cardanol were highly overlapped in the chemical shift rang of 7.97–38.08 ppm.35,36 Other chemical shifts (ppm) were the aromatic carbon resonances: C5, C6, C7, C8, and C9 were highly overlapped in the chemical shift rang of 111.46–143.04 ppm.37 In addition, X-ray photoelectron spectroscopy (XPS) analysis was performed on the surfaces of CBCP cured by heating at 200 °C for 2 h and CBCP catalyzed by CuCl2, see Fig. S2(a–h).† These chemical shifts of the carbons confirm the CBCP was successfully prepared.
Since the crosslinking degrees of polymers vary with heating temperature, the physical and mechanical properties of polymer coatings may also vary with temperature. In this work, CBCP was heated at different temperatures for 2 h, and its physical and mechanical properties were tested accordingly (Table 1). Eqn (1) was used to calculate the gelling rate:
The gel rate = (m1/m2) × 100% | (1) |
Properties | a | b | c | d | e | F | g | h | i | |
---|---|---|---|---|---|---|---|---|---|---|
25 °Ca | 40 °C | 60 °C | 80 °C | 100 °C | 120 °C | 140 °C | 160 °C | 180 °C | ||
a Coatings not heated and placed for two weeks before testing.b Time for coatings to completely dissolve in xylene. | ||||||||||
Pencil hardness | 2H | B | B | 2H | 4H | 6H | 6H | 6H | 6H | |
Impact strength (g cm−1) | Obverse | 50000 | 50000 | 35000 | 25000 | 20000 | 15000 | 15000 | 15000 | 15000 |
Reverse | 50000 | 35000 | 15000 | 15000 | 15000 | 15000 | 15000 | 15000 | 15000 | |
Adhesive force (grade) | Circle | 1 | 1 | 1 | 1 | 2 | 2 | 2 | 3 | 3 |
Cross | 0 | 0 | 0 | 0 | 1 | 1 | 2 | 3 | 3 | |
Flexibility (mm) | 2 | 2 | 2 | 2 | 10 | 10 | 10 | 10 | 10 | |
The gel rate (%) | 73 | 0.5 hb | 0.5 hb | 62 | 92 | 100 | 100 | 100 | 100 |
Therefore, CBCP was tested after dried at room temperature two weeks and the results showed gelling rate reaching 73% and pencil hardness is 2H. Also, no discoloration of solvent or coating dissolution took place. The results also revealed excellent impact strength, adhesion, and flexibility of this material dried naturally. By comparison, though the hardness and gel rate of CBCP can be improved by increasing the heating temperature, features like impact strength, adhesion and flexibility may constantly reduce. Here, naturally dried CBCP coating at room temperature underwent orderly and slow cross-linking polymerization, enabling better balanced internal structure to cope with the damage caused by external forces.
The structure of PDPI and NDPI was further characterized by solid-state 13C CP/MAS NMR, as shown in Fig. 5. The peaks at 165.42 (A) and 162.33 (B) ppm correspond to the resonances of carbonyl carbons on an amide (C1) of PDPI (A) and NDPI (B) respectively.40 Other chemical shifts (ppm) were the aromatic carbon resonances: C2, C3, C4 C5 C6, C7, and due to the aromatic carbons on benzidine (C5, C6, C7) have similar chemical environments were highly overlapped in the chemical shift rang of 110.35–121.81 ppm.41 In addition, on account of NDPI has more aromatic carbons (C2, C3, C8) than PDPI, the integral area ratios of C2 and C3 in NDPI were significantly higher and overlapped.42 All the results indicating the successful preparation of PDPI and NDPI. The surface morphology of corrosion inhibitors in Fig. S1† revealed the two-dimensional sheet structures of PDPI and NDPI and the mobility test for water and solvent resistance of PDPI and NDPI in Fig. S3.†
(2) |
In Tafel curves, the current corresponding to the intersection of the slope of anode and cathode curves represented the corrosion current (Icorr). The slopes of both anode and cathode curves ba and bc were obtained by fitting analysis of the testing software.
(3) |
(4) |
In general, the corrosion degree of each coating can preliminarily be evaluated though Icorr and E in Tafel curves.25 The coatings with lower Icorr and higher E exhibited better corrosion resistance. In 3.5 wt% NaCl solution, the corrosion resistance of bare copper was poor. By comparison, the samples protected by coatings all showed excellent corrosion resistance (Fig. 6(a)). As shown in Table 2, the different values of Rp, PE, and CR, indicating variable corrosion resistances. Compared to bare copper, the Icorr of CBCP coating decreased to 1.369 × 10−8 A cm−2 and E increased to −0.2585 V. The Rp of CBCP was 1.120 × 108 Ω, CR was 1.672 × 10−4 mm year−1, and PE of metal was 99.82%. Hence, CBCP possessed good corrosion resistance performance when coated on the metal substrate.
Fig. 6 Tafel curves of different coatings in (a) 3.5 wt% NaCl solution and (b) 1 M HCl aqueous. Bare copper (M), CBCP (O), CP-01 (A), CP-05 (B), CP-10 (C), CN-01 (D), CN-05 (E), and CN-10 (F). |
Samples | E (V) | Icorr (A cm−2) | Rp (Ω) | PE (%) | CR (mm year−1) | |
---|---|---|---|---|---|---|
a 0 – based on this sample; — – excluded this sample. | ||||||
Bare copper | −0.3160 | 7.914 × 10−6 | 2.487 × 105 | 0a | —a | 9.666 × 10−2 |
CBCP | −0.2585 | 1.369 × 10−8 | 1.120 × 108 | 99.82 | 0 | 1.672 × 10−4 |
CP-01 | −0.4460 | 3.659 × 10−9 | 3.035 × 108 | 99.96 | 73.28 | 4.469 × 10−5 |
CP-05 | −0.2042 | 2.764 × 10−10 | 3.874 × 109 | 99.99 | 97.98 | 3.376 × 10−6 |
CP-10 | −0.3470 | 7.580 × 10−10 | 1.720 × 109 | 99.99 | 94.46 | 9.259 × 10−6 |
CN-01 | −0.2620 | 3.083 × 10−9 | 5.414 × 108 | 99.96 | 77.48 | 3.765 × 10−5 |
CN-05 | −0.1830 | 3.373 × 10−10 | 3.385 × 109 | 99.99 | 97.54 | 4.120 × 10−6 |
CN-10 | −0.3280 | 5.112 × 10−10 | 2.183 × 109 | 99.99 | 96.26 | 6.244 × 10−6 |
Proper amount of corrosion inhibitor could enhance the corrosion resistance of coatings. Here, the Icorr and CR of composite coatings were lower than those of CBCP coatings, and protection efficiency greater than 70% when compared to CBCP (Table 2). Both CP-05 and CN-05 showed excellent corrosion resistance, with Icorr to 2.764 × 10−10 A cm−2 and 3.373 × 10−10 A cm−2, CR calculated as 3.376 × 10−6 mm year−1 and 4.120 × 10−6 mm year−1 and Rp valued to 3.874 × 109 Ω and 3.385 × 109 Ω, respectively. Compared to CBCP, the protection efficiency (PE) of CP-05 and CN-05 reached values of 97.98% and 97.54%, respectively. Also, PE reached 99.9% when compared to bare copper. Overall, the corrosion resistance of CBCP coating significantly improved after the introduction of polyimide.
The Tafel curves of composite coatings were also investigated in different media, and then, 1 M HCl solution as the corrosive medium. Fig. 6(b) and Table 3 showed the Tafel curves and parameters of the coatings in 1 M HCl solution, respectively. The anti-corrosion performance of the coatings in acidic media was slightly worse than in neutral media. However, the anti-corrosion effects of the composite coatings were still remarkable. Compared to CBCP, the PE values of CP-05 (B) and CN-05 (E) reached 94.87% and 93.24%, respectively. Both CP-10 (C) and CN-10 (F) showed similar performances in acidic media as in neutral media. Also, their corrosion resistances decreased slightly when compared to CP-05 (B) and CN-05 (E). Therefore, excess amounts of polyimide inhibited the anticorrosion effect of the coatings. When polyimide was not evenly dispersed in CBCP, the compactness of the coatings became compromised, thereby weakening the protective ability of the coatings on metal materials.
Sample | E (V) | Icorr (A cm−2) | Rp (Ω) | PE (%) | CR (mm year−1) |
---|---|---|---|---|---|
a 0 – based on this sample. | |||||
CBCP | −0.210 | 6.009 × 10−7 | 1.347 × 106 | 0a | 7.340 × 10−3 |
CP-01 | −0.210 | 2.447 × 10−7 | 1.407 × 106 | 59.28 | 2.989 × 10−3 |
CP-05 | −0.028 | 3.080 × 10−8 | 4.121 × 107 | 94.87 | 3.762 × 10−4 |
CP-10 | −0.068 | 8.146 × 10−8 | 1.049 × 107 | 86.44 | 9.945 × 10−4 |
CN-01 | −0.229 | 2.511 × 10−7 | 5.275 × 106 | 58.21 | 3.067 × 10−3 |
CN-05 | −0.078 | 4.601 × 10−8 | 2.556 × 107 | 93.24 | 5.620 × 10−4 |
CN-10 | −0.183 | 8.724 × 10−8 | 1.180 × 107 | 81.23 | 1.066 × 10−3 |
Some of the best anti-corrosion coatings reported in literature were prepared with cardanol-based composite coatings, and the PE values of the two-dimensional lamellar polyimide/cardanol-based benzoxazine copper polymer composite coatings prepared here were compared with other results in literature in Table 4. Among previously reported coatings, the best PE value of 99.87% was reported for a 5 wt% HTCP/SBCBz-EP/MS composite coating (SBCBz-EP: siloxane-based cardanol benzoxazine–epoxy). Notably, the PE value of the two-dimensional lamellar polyimide/cardanol-based benzoxazine copper polymer composite coating (CP-05) in this work increased by 99.99% compared with bare copper and 97.98% compared with the pure matrix (CBCP), both of which were significantly better than previous coatings reported in literature. In conclusion, the combination of polyimide and cardanol-based benzoxazine copper polymer significantly improves the protection efficiency of the coating.
To study the influence of polyimide corrosion inhibitors, the corrosion resistance of different coatings CBCP (O), CP-01 (A), CP-05 (B), CP-10 (C), CN-01 (D), CN-05 (E) and CN-10 (F) were evaluated by EIS in 3.5 wt% NaCl solution for 1–120 h. In Fig. 7, the capacitance arcs in the low/high-frequency region were related to the transfer and charge transfer of corrosion reaction.25 Therefore, the corrosion resistance of the coatings can be judged by the diameters of the curves. The local EIS spectrograms revealed all coatings with large capacitive arcs at the initial stage of immersion. The capacitance arcs of CP-05 (B), CP-10 (C), CN-05 (E), and CN-10 (F) looked relatively large, indicating better corrosion resistance. By comparison, the capacitance arcs of CBCP were the smallest, consistent with the results of Tafel polarization. As testing time increased, the diameters of all capacitive arcs decreased. The reason for this had to do with the continuous erosion of the coatings by the corrosive medium, which resulted in holes and cracks, as well as partial rupture of the protective layer. At the test times of 96 h and 120 h, the materials CP-10 (C), CN-05 (E) and CN-10 (F) showed multiple capacitive arcs with small radii in the high-frequency region. Thus, the corrosive medium penetrated the coatings through some aperture, but did not yet reach the surface of the metal, keeping it protected.52 CP-05 (B) still showed a large capacitive arc resistance, revealing excellent corrosion resistance. Polyimide compound benzoxazine resin as a protective layer of metal materials could effectively delay the infiltration of water and other corrosive media, thereby preventing the metal from corrosion.
Fig. 7 Nyquist plots of different coatings in 3.5 wt% NaCl solution. CBCP (O), CP-01 (A), CP-05 (B), CP-10 (C), CN-01 (D), CN-05 (E), and CN-10 (F). |
The changes in EIS Bode plots of the coatings immersed in 3.5 wt% NaCl solution were illustrated in Fig. 8. The Bode plots revealed CP-05 (B) with only one time constant in the late test period. It also maintained a high impedance modulus over a wide frequency range. Low-frequency impedance modulus (|Z|f = 0.01 Hz) was often used to evaluate the corrosion resistance of coatings.53 CP-05 (B) showed a high impedance modulus in the low-frequency region of Bode plots, indicating the good corrosion resistance of the coating. The composite coatings showed good anticorrosion properties, mainly in the following aspects (as shown in Fig. 9): firstly, the higher cross-linking density cardanol-based benzoxazine film was responsible for the good shielding effect. Secondly, though corrosive mediums are known to easily penetrate coatings through tiny surface cracks, two-dimensional lamellar polyimide can effectively avoid and prevent it from accessing the metal surface. PDPI or NDPI that played an important role in the maze effect and reduction the corrosion rate of the copper pieces. Thirdly, the nitrogen atom of organic amine compounds usually has lone pairs of electrons, which can form coordination bonds with the hollow d orbitals of the metal, such that the molecule adsorbed on the metal surface forms a layer of protective film to protect the metal.54
Fig. 8 Bode plots of different coatings in 3.5 wt% NaCl solution. PBzn (O), P1-01 (A), P1-05 (B), P1-10 (C), P2-01 (D), P2-05 (E), and P2-10 (F). |
The surface morphologies of different coatings in 3.5 wt% NaCl solution for 120 h were gathered in Fig. 10. The surface of CBCP coating looked smoother and flatter, while the composite coatings revealed relatively rough surfaces. This might be related to the dispersion of polyimide in CBCP. Serious corrosion pits and holes appeared on CBCP surface after corrosion since incomplete cross-linking of CBCP may result in rapid penetration of the coatings by the corrosive media. The composite coatings did not exhibit large holes, but many small corrosion pits and holes were noticed. Since the added amounts of the corrosion inhibitors in CP-01 (A) and CN-01 (D) were small, they were incapable of completely shielding the corrosive media. On the other hand, large numbers of corrosion pits existed on coatings surfaces though CP-10 (C) and CN-10 (F) showed some small holes after 120 h immersion in 3.5 wt% NaCl solution, indicated the presence of corrosion inhibitors enhanced corrosion resistance. The corrosion resistance of CP-10 (C) and CN-10 (F) may be caused by excess added amounts, resulting in uneven dispersion of corrosion inhibitors in the solvent.55 CP-05 (B) showed excellent anticorrosion performances in all composite coatings with no obvious corrosion holes and only some corrosion pits. Therefore, CP-05 (B) exerted a good shielding effect on the metal in corrosive media when compared to coatings, showing excellent anti-corrosion performance.
Fig. 10 SEM images of different coatings immersed in 3.5 wt% NaCl solution for 120 h. CP-01 (A), CP-05 (B), CP-10 (C), CN-01 (D), CN-05 (E), CN-10 (F), and CBCP (O). |
THRI = 0.49 × [T5 + 0.6 × (T30 − T5)] | (5) |
Samples | 5% weight loss [T5] (°C) | 30% weight loss [T30] (°C) | THRI (°C) | Char yield at 600 °C (%) |
---|---|---|---|---|
CN-05 | 245.3 | 392.6 | 163.5 | 30.1 |
CP-05 | 240.6 | 387.3 | 161.0 | 29.2 |
CBCP | 240.4 | 372.1 | 156.5 | 22.4 |
The data relating to 5% weight loss temperature, 30% weight loss temperature, and carbon residue rate at 600 °C of all three coatings were listed in Table 5. The temperature corresponding to a weight loss rate of 5% can be considered as the initial decomposition temperature of the coatings and the low-molecular weight oligomers were volatilized.61 The difference in thermal stability of the coatings was most obvious at a weight loss rate of around 50%. As temperature rose to 600 °C, the carbon residue rates of CBCP, CP-05, and CN-05 reached 22.4%, 29.2% and 30.1%, respectively. The reason for this result might be the small anti-corrosion inhibitor added amounts that led to no obvious differences in heat resistance between the composite coatings. Therefore, the addition of PDPI and NDPI effectively improved the thermal stability and carbon residue rate of CBCP. The high decomposition temperature of composite coatings would greatly help practical applications.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d1ra08844k |
This journal is © The Royal Society of Chemistry 2022 |